CSWIP 3.0/3.

1 ACCEPTANCE LEVELS
SPECIFICATION BW/VI/00

PLATE ONLY
Key

L = Length of defect D = Depth or height of defect


W = Width of defect {applicable to inclusions only}
# 1 2 3 4 5

DEFECT NAME Excess penetration* Undercut Angular misalignment Arc strike / Stray flash Linear misalignment

6 7 8 9 10 11 12 13 14

Cracks Overlap Lack of side wall fusion Porosity / Gas Pores / Elongated gas cavities, pipes Lack of root fusion Lack of root penetration Root concavity Incomplete filled groove Excess weld metal*

MAXIMUM ALLOWANCE 2.0 mm D maximum 10% up to maximum D 1.5 mm Accept Not permitted Maximum D t < 10 mm 0.8 mm t > 10 mm 1.0 mm Not permitted Accumulative total for both shall not 25 mm in weld face exceed 30 mm length Maximum dimension of any area or individual (as applicable) Accumulative total for both defects shall not exceed 30 mm 1.5 mm 25 mm in root length Maximum D 1 mm Not permitted 2 mm D maximum

REMARKS

15 16

Mechanical damage Inclusions (slag/silica etc.)

Smooth transition required. All runs shall blend smoothly. No lack of interun fusion Dependent on depth and blend Accumulative total shall not exceed 20 mm L in weld length (root & face independent)

Seek advice Individual maximum L < 12 mm W < 3mm

* When linear misalignment is present the following shall be applied.


Excessive weld metal: Maximum height to be measured from a direct line from lowest plate, across weldment. Excessive penetration: Maximum height to be measured from lowest plate.

WIS 5-ARPP Issue 3 Date: 28/05/03