Download as pdf or txt
Download as pdf or txt
You are on page 1of 1

TROUBLESHOOTING

JETTING

Fault category
Streaking

Alternative terms

Description
Generally serpentine strand of the melt first injected into the mould, found near the sprue or at constricted sections, and visible on the part surface

Possible Causes 1. Unsuitable design of gate or narrow sections preventing laminar flow. Gate position with no opposing wall. Gate cross section or narrow section too small 2. Injection speed too high

Remedial Actions Redesign gate. Position gate opposite a wall. Enlarge gate cross section. Redesign changes in cross section Inject material slowly at first, then switch to a faster speed

Notes
Occurs more frequently with amorphous products because of their higher viscosity and lower elongation