PSL 1 and PSL 2 differ in several parameters according to API 5L 43rd Edition. PSL 1 allows for repair by welding of pipe body, plate, and skelp without filler metal. It has a smaller grade and size range than PSL 2. PSL 1 requires heat treatment of electric welds only for grades above X42, has higher maximum carbon contents, and does not require fracture toughness testing or non-destructive inspection of seamless pipes. Traceability is only required until tests are passed under PSL 1. In contrast, PSL 2 has more stringent requirements for welding methods, heat treatment, chemical compositions, testing, inspection, certification and traceability.
PSL 1 and PSL 2 differ in several parameters according to API 5L 43rd Edition. PSL 1 allows for repair by welding of pipe body, plate, and skelp without filler metal. It has a smaller grade and size range than PSL 2. PSL 1 requires heat treatment of electric welds only for grades above X42, has higher maximum carbon contents, and does not require fracture toughness testing or non-destructive inspection of seamless pipes. Traceability is only required until tests are passed under PSL 1. In contrast, PSL 2 has more stringent requirements for welding methods, heat treatment, chemical compositions, testing, inspection, certification and traceability.
PSL 1 and PSL 2 differ in several parameters according to API 5L 43rd Edition. PSL 1 allows for repair by welding of pipe body, plate, and skelp without filler metal. It has a smaller grade and size range than PSL 2. PSL 1 requires heat treatment of electric welds only for grades above X42, has higher maximum carbon contents, and does not require fracture toughness testing or non-destructive inspection of seamless pipes. Traceability is only required until tests are passed under PSL 1. In contrast, PSL 2 has more stringent requirements for welding methods, heat treatment, chemical compositions, testing, inspection, certification and traceability.
Parameter PSL 1 PSL 2 Ref: API 5L 43rd Edition Repair by welding of pipe body plate,and skelp Repair by welding of weld seams without ller metal Grade range Size range Type of ends Seam welding Electric welds: welder frequency Heat treatment of electric welds Chemistry: Max C for Seamless pipe Chemistry: Max C for Welded pipe Chemistry: Max P Chemistry: Max S Carbon equivalent: Yield strength, maximum UTS (Ultimate Tensile Strength) maximum Fracture toughness Non-destructive inspection of Seamless Certication Traceability A25 through X70 0.405" through 80" Plain end, Threaded end, Bevelled end special coupling pipe All methods: continuous welding limited to A25 No minimum Required for grades >X42 0.28% for grades B 0.26% for grades B 0.030% for grades A 0.03% Only when purchaser species SR18 None None None required Only when purchaser species SR4 Traceable only until all tests are passed Permitted by agreement Permitted Traceable only until all tests are passed unless SR15 is specied B through X80 4.5" through 80" Plain end All methods: except continuous welding and laser welding kHz minimum 100 Required for all grades (B through X80) 0.24% 0.22% 0.03% 0.02% Maximum required for each grade Maximum for each grade Maximum for each grade Required for all grades SR4 mandatory Prohibited Prohibited Certicates (SR15.1) mandatory Traceable after completion of tests (SR15.2) mandatory Table 1 Table 1 Table 1 Table 1 5.1.3.3.2 5.1.3.3.1; 5.1.3.3.2; 6.2.7 Tables 2A, 2B Tables 2A, 2B Tables 2A, 2B Tables 2A, 2B 4.2; 4.3; 6.1.3; SR15.1 Tables 3A, 3B Tables 3A, 3B 6.2.6; 9.3.5; 9.8.4; 9.10.7; Table 14 9.7.2.6 5.3.2; 9.7.6; B.1; B.2 4.3; 9.7.4.4; 9.7.6; B.1.1; B.4 12.1 5.6 (Based on API 5L Edition 43) ERA ENERGY