STORAGEANDDRYINGCONTROLPROCEDURE

Diagramofdryingconditionsforlowhydrogenelectrodes(FIGURE1)

Normalpackingkeptinstorage

BAKINGOVEN
3Hours,350Cforthe1stcycle
nd

rd

2Hours,350Cforthe2 and3 cycles

st

nd

rd

1 cycle2 and3 cycles

VacPacelectrodes
Fromstorage

HOLDINGOVEN1
150C
Remaining
electrodes

HEATEDQUIVERS
100C

Note
(Onthefield)

Issueforuse

WetordamagedElectrodes

BendandDiscard

NoteRemainingelectrodesshallbereturnedtobakingovensandredried.Baking
operationswillberepeateduptoamaximumofthree(3)cyclesafterwhichelectrodes
shallbebentanddiscarded.

Thenumberofredryingcyclesshallbecontrolledbypaintmarkingthestudendof
Returnedelectrodesasfollows:

2ndredryingcyclewhitepaintonelectrodestubend

3rdredryingcycleredpaintonelectrodestubend

STORAGEANDDRYINGCONTROLPROCEDURE

DiagramofstorageconditionsforcelluloseelectrodesAndRutile
(FIGURE2)
(Rutile,1hourfor120degreedasperAws5.1specifications)

Normalpackingkeptinstorage

HOLDINGOVEN2
4050C

Remaining
electrodes

IssueforUse

WetorDamaged
Electrodes

BendandDiscard