Professional Documents
Culture Documents
GB Grade Asp 2060
GB Grade Asp 2060
CHEMICAL COMPOSITION
ASP 2060
GUIDELINES FOR HARDENING
Cr
Mo
Co
2.30
4.2
7.0
6.5
10.5
6.5
STANDARDS
Europe: HS 6-7-6-10
Germany: W.Nr. 1.3241
DELIVERY HARDNESS
Soft annealed max. 340 HB
DESCRIPTION
HRC
72
70
68
66
64
62
1180
60
1150
58
1100
56
520
1050
1000
540
560
580
600
620 C
Tempering Temperature
Tempering time 3x1 hour at 560C
CCT CURVE
APPLICATIONS
FORM SUPPLIED
Round bars
Forged bars
Flat & square bars
Tool bit sections
HEAT TREATMENT
PROCESSING
GRINDING
The above is for information only and does not create any binding contractual obligations
ASP is a registered trademark of Erasteel
PDS_ASP2060_EN_V1_2012
SURFACE TREATMENT
Nm
12
Rmb
PROPERTIES
PHYSICAL PROPERTIES
Temperature
Density
g/cm3 (1)
Modulus of elasticity
kN/mm2 (2)
Thermal expansion
ratio
per C (2)
Thermal conductivity
W/mC (2)
Specific heat
J/kg C
(2)
400C
600C
7.9
7.9
7.8
222
Reb
6
Tot.work
20C
250
10
0
950
1000
1050
1100
1150
Hardening Temperature in C
200
Original dimensions 6 mm
Tempering 3 x 1 hour at 560C
Dimensions of test piece 4.7 mm
10.6x10-6 11.1x10-6
24
28
27
420
510
600
0
1200 C
(1)=Soft annealed
(2)=Hardened 1180C and tempered 560C, 3x1 hour
IMPACT STRENGTH
Nm
HRC
24
70
21
69
Impact energy
18
68
15
67
12
66
65
6
3
0
950
64
Hardness
1000
1050
63
1100
1150
Hardening Temperature in C
Original dimensions 9 x 12 mm
Tempering 3 x 1 hour at 560 C
Unnotched test piece 7 x 10 x 55 mm
62
1200 C
COMPARATIVE PROPERTIES
Machinability
Wear
resistance
E M2
E M35
E M42
C8
E M3:2
M9V
E M7
WKE 42
WKE 45
ASP 2005
ASP 2015
ASP 2017
ASP 2023
ASP 2030
ASP 2052
ASP 2053
ASP 2060
Toughness
Hot
hardness
Grindability