17-4 PH STEEL
STAINLESS
UNS S17400
17-4 PH-S-8-01-07
AK STEEL 17-4 PH STAINLESS STEEL DATA SHEET
MECHANICAL PROPERTIES
Typical Mechanical Properties* common member of the class and is gen-
erally considered to have the best
Condition
Property A H 900 H 925 H 1025 H 1075 H 1150 H 1150-M weldability. When a weld filler is needed,
AWS E/ER 630 is most often specified.
UTS, ksi 160 210 200 185 175 160 150 AK Steel 17-4 PH Stainless Steel is well
(MPa) (1103) (1448) (1379) (1276) (1207) (1103) (1034)
known in reference literature and more
0.2% YS, ksi 145 200 195 170 165 150 130 information can be obtained in this way.
(MPa) (1000) (1379) (1345) (1172) (1148) (1034) (896)
Elongation, 5.0 7.0 8.0 8.0 8.0 11.0 12.0 SPECIFICATIONS
% in 2" Specifications are listed without revision
(50.8 mm) indications. Contact ASTM Headquarters
Hardness, C35 C45 C43 C38 C37 C35 C33 for latest ASTM revision. For AMS revi-
Rockwell sion, contact AMS Division of SAE.
*Cold-flattened sheets and strip.
AMS 5604 Sheet, Strip and Plate
PHYSICAL PROPERTIES ASTM A 693 Plate, Sheet and Strip
Condition Condition Condition Condition (Listed as Grade 630-UNS S17400)
A H 900 H 1075 H 1150
(Magnetic) (Magnetic) (Magnetic) (Magnetic)
METRIC CONVERSION
Density, lbs/in (g/cm )
3 3
0.28 (7.78) 0.282 (7.80) 0.283 (7.81) 0.284 (7.82) Data in this publication are presented in
Electrical Resistivity,
U.S. customary units. Approximate
microhm-cm 98 77 metric equivalents may be obtained by
performing the following calculations:
Specific Heat 0.11 (0.46) 0.11 (0.46)
BTU/lb/ F (32 - 212F) Length (inches to millimeters)
kJ/kgK (0 - 100oC) Multiply by 25.4
Thermal Conductivity
BTU/hr/ft2/in/F (W/mK) Strength (ksi to megapascals or
300F (149C) 124 (17.9) meganewtons per square meter)
500F (260C) 135 (19.5) Multiply by 6.8948
900F (482C) 157 (22.6)
Temperature (Fahrenheit to Celsius)
Mean Coefficient of Thermal Expansion (Fahrenheit - 32) Multiply by 0.5556
in/in/F (m/mK)
100 - 70F (-73 - 021C) 5.8 x 10-6 (10.4) 6.1 x 10-6 (11.0) Density (pounds per cubic inch to
70 - 200F (21 - 093C) 6.0 x 10-6 (10.8) 6.0 x 10-6 (10.8) 6.3 x 10-6 (11.3) 6.6 x 10-6 (11.9) kilograms per cubic meter) Multiply
70 - 600F (21 - 316C) 6.2 x 10-6 (11.2) 6.3 x 10-6 (11.3) 6.6 x 10-6 (11.9) 7.1 x 10-6 (12.8)
by 27,670
70 - 800F (21 - 427C) 6.3 x 10-6 (11.3) 6.5 x 10-6 (11.7) 6.8 x 10-6 (12.2) 7.2 x 10-6 (13.0)
WELDABILITY required to achieve optimum mechanical
The information and data in this product data sheet are
The precipitation hardening class of stain- properties by considering the best heat- accurate to the best of our knowledge and belief, but are
intended for general information only. Applications sug-
less steels is generally considered to be treated conditions in which to weld and gested for the materials are described only to help readers
weldable by the common fusion and resis- which heat treatments should follow make their own evaluations and decisions, and are neither
guarantees nor to be construed as express or implied
tance techniques. Special consideration is welding. This particular alloy is the most warranties of suitability for these or other applications.
AK Steel Corporation
9227 Centre Pointe Drive
West Chester, OH 45069
www.aksteel.com