Professional Documents
Culture Documents
VDU Velocity Steam Line
VDU Velocity Steam Line
VDU Velocity Steam Line
Doc. NO F/09/01
Inspection Report
Page No.
ISSUE/REV. NO 1/00
Observation:
These exchangers are having a history of frequent leakages from August 2013 onwards and
inspection of these bundles has revealed scaling and thinning from outside and cooling water
deposits inside the tubes.
Tube failure details are as follow:
13-EE-AS-103A 13-EE-AS-103B
August 2013 Scaling & thinning from tube OD,
One tube found leaky
September 8 tubes found leaky other 10
2013 thinned tubes were also plugged
July 2014 Tube bundle replaced with new
spare bundle & painting of cooling
water side components done
TA 2015 No significant observation No significant observation
August 2017 After leakage bundle replaced with
repaired spare bundle with 8 tubes
plugged. Cooling water deposits
were observed inside the tubes
November External scaling on tubes, thinning
2017 and tubes found choked from inside
1
BORL
Doc. NO F/09/01
Inspection Report
Page No.
ISSUE/REV. NO 1/00
Photographs
2
BORL
Doc. NO F/09/01
Inspection Report
Page No.
ISSUE/REV. NO 1/00
Image showing cooling water fills observed after opening of channel head
Conclusion:
Shell side fluid is corrosive in nature because of presence of H2S, HCl and water
causing the scaling and under deposit corrosion of tubes from OD.
There is less flow/stagnation of cooling water inside the tubes causing the MIC/under
deposit corrosion.
Cooling Tower fills choked the tubes and caused the stagnation resulting in severe
deposition.
Recommendation:
Close control and monitoring of shell side fluid pH to control the corrosion rate.
Fills kind of things which can choke the tubes or reduce the flow of cooling water shall
not be allowed to reach to the exchanger tubes.
Proper flow of cooling water shall be maintained in all the tubes.
3
BORL
Doc. NO F/09/01
Inspection Report
Page No.
ISSUE/REV. NO 1/00
Shell Tube
Fluid circulated LGO Product Cooling water
Working pressure (Kg/cm2) 11.4 4
Working 65/40 33/45
Temperature(in/out) 0C
Design Pressure(Kg/cm2) 23.7 18.2
Design Temperature 0C 80 85
MOC SA-516 Gr60 SA-179
4
BORL
Doc. NO F/09/01
Inspection Report
Page No.
ISSUE/REV. NO 1/00
Conclusion: Since this exchanger is in the ground floor and hence there should not be any
stagnation/less flow issue still severe deposition (tubercles) has been observed inside the
tubes which indicates that tubes were not getting the enough flow. Also lab analysis of the
tube side deposit indicates high percentage of hydrocarbon in it.
Recommendation:
5
BORL
Doc. NO F/09/01
Inspection Report
Page No.
ISSUE/REV. NO 1/00
Proper flow of cooling water to be maintained inside the tubes to avoid stagnation.
Effectiveness of cooling water treatment and dosing system to be checked properly.
In TA’18 effective cleaning of tubes to be carried out to facilitate inspection and RFET
for assessing the health of tube bundles.