Guiding Formulation

for the production of a silver hammer finish powder coating via direct
extrusion of PowderSafe® 1080-01 Silver

Rec. No. Date Revised: page 1 of 1


41-09002 23.01.13

Binder / Hardener
1. Araldite GT 6063 45,8 www.huntsman.com
2. Crylcoat 1540-0 45,8 www.cytec.com

Pigment / Extender
3. Blanc Fixe N 6,0 www.solvay-bariumstrontium.com
®
4. PowderSafe 1080-01 Silver 2,0 www.eckart.net

Additive
5. Ceraflour 961 0,2 www.byk.com
6. Ceraflour 967 0,2 www.byk.com
----------
100,0

Processing instruction for the production of a silver hammer finish powder coating via direct extrusion
of PowderSafe® 1080-01 Silver:

Premix Pos. 1-6 1 min, 1500 rpm


Extruder twin screw Prism TSE 16
heating zone 110°C
shaft speed 350 rpm
Cooling drum
Micronising Retsch ZM 100 16000 rpm
Sieving shaking sieve mw = 125 µm DIN 4188

Application :

Substrate Q-panels aluminium A-36 152 x 76 x 0,5mm


Powder gun 80 kV / 2,0 bar
Curing 10 min at 200°C circulated air temp.

This information is for your advice on conscientiously ECKART GmbH


executed tests. Considering the variety of tests this Guentersthal 4
information is without warranty. 91235 Hartenstein
Germany
Fax: +49 (0) 91 52-77- 45 09
Tel.: +49 (0) 91 52-77- 45 -10 or -11