Professional Documents
Culture Documents
Shift Conversion Catalysts - Operating Manual
Shift Conversion Catalysts - Operating Manual
Shift Conversion Catalysts - Operating Manual
Upload
Login
Signup
Home
Explore
Presentation Courses
PowerPoint Courses
by LinkedIn Learning
Search
Successfully reported this slideshow.
We use your LinkedIn profile and activity data to personalize ads and to show you more relevant ads. You can change your ad preferences anytime.
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 1/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 2/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 3/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 4/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 5/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 6/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 7/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 8/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 9/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 10/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 11/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 12/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 13/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 14/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 15/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 16/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 17/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 18/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 19/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 20/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 21/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 22/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 23/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 24/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 25/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 26/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 27/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
Upcoming SlideShare
Loading in …5
×
12 of 28
Share
Like
Download
...
...
Published in: Technology
2 Comments
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 28/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
17 Likes
Statistics
Notes
Full Name
Comment goes here.
12 hours ago Delete Reply Block
Are you sure you want to Yes No
Your message goes here
Consuelo Russo
Increasing Sex Drive And Getting Harder Erections, Naturally ♣♣♣ http://t.cn/Ai88iYkP
2 weeks ago Reply
Are you sure you want to Yes No
Your message goes here
Aurora Brennan
Is Your Ex With a Woman? Don't lose your Ex boyfriend! This weird trick will get him back! ◆◆◆ http://ishbv.com/exback123/pdf
2 months ago Reply
Are you sure you want to Yes No
Your message goes here
Gopi Krish
1 month ago
Vignesh Cg
6 months ago
NanLiu38
7 months ago
NithinManoj1
7 months ago
ThausifRahman
8 months ago
Show More
No Downloads
Views
Total views
11,697
On SlideShare
0
From Embeds
0
Number of Embeds
16
Actions
Shares
0
Downloads
605
Comments
2
Likes
17
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 29/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
Embeds 0
No embeds
No notes for slide
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 31/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
appropriate occupational exposure limits should be strictly observed. If these limits are likely to be exceeded then respiratory protection should be used. Everyone
involved in the handling operation should clean up afterwards and, in particular must wash before eating. Clothing should be changed at the end of each shift, and
more frequently if contamination is heavy. Ergonomics Physical hazards arise from the handling of drums, material and lifting equipment. Personnel should be
aware of these and appropriate precautions taken.
12. 12. Refinery Process Stream Purification Refinery Process Catalysts Troubleshooting Refinery Process Catalyst Start-Up / Shutdown Activation Reduction In-situ
Ex-situ Sulfiding Specializing in Refinery Process Catalyst Performance Evaluation Heat & Mass Balance Analysis Catalyst Remaining Life Determination
Catalyst Deactivation Assessment Catalyst Performance Characterization Refining & Gas Processing & Petrochemical Industries Catalysts / Process Technology -
Hydrogen Catalysts / Process Technology – Ammonia Catalyst Process Technology - Methanol Catalysts / process Technology – Petrochemicals Specializing in the
Development & Commercialization of New Technology in the Refining & Petrochemical Industries Web Site: www.GBHEnterprises.com Reduction and start-up of
VULCAN Series VSG-F101 When the reactor has been charged the high temperature shift catalyst must be reduced before it can be used. The reduction of high
temperature shift catalyst is invariably carried out with process gas under conditions that allow the haematite to be converted to magnetite without further reduction
to metallic iron. Reduction also converts any of the small quantity of residual hexavalent chromium (CrO3) to trivalent chromium (Cr2O3). 3Fe2O3 + H2 → 2
Fe3O4 + H2O ΔH = -16.3 kJ/mol 3Fe2O3 + CO → 2 Fe3O4 + CO2 ΔH = +24.8 kJ/mol 2CrO3 + 3H2 → Cr2O3 + 3H2O ΔH = -684.7 kJ/mol 2CrO3 + 3CO →
Cr2O3 + 3CO2 ΔH = -808.2 kJ/mol It is very important that steam should be present during the reduction procedure in order to prevent over-reduction of the
catalyst. It can be shown that if the H2O/H2 ratio exceeds 0.18 at 400o C (750o F) or 1.0 at 550o C (1020o F) then the desired magnetite is the stable phase.
Similarly, the CO2/CO ratio should exceed 1.16 at 400o C (750o F) or 1.0 at 550o C (1020o F). The graph below summarizes the conditions necessary to prevent
the reduction of Fe3O4 to metallic iron in hydrogen and steam mixtures. Figure 1 Minimum H2O to H2 Ratio for HTS Catalyst Reduction
13. 13. Refinery Process Stream Purification Refinery Process Catalysts Troubleshooting Refinery Process Catalyst Start-Up / Shutdown Activation Reduction In-situ
Ex-situ Sulfiding Specializing in Refinery Process Catalyst Performance Evaluation Heat & Mass Balance Analysis Catalyst Remaining Life Determination
Catalyst Deactivation Assessment Catalyst Performance Characterization Refining & Gas Processing & Petrochemical Industries Catalysts / Process Technology -
Hydrogen Catalysts / Process Technology – Ammonia Catalyst Process Technology - Methanol Catalysts / process Technology – Petrochemicals Specializing in the
Development & Commercialization of New Technology in the Refining & Petrochemical Industries Web Site: www.GBHEnterprises.com During catalyst reduction
it is preferable to avoid the condensation of water in the catalyst bed. If possible, therefore, the catalyst should be heated in an inert gas stream to a temperature that
will prevent the condensation of steam before process gas is admitted to the reactor. All HTS catalysts contain a small amount of residual sulfate that is converted to
H2S during the reduction procedure. Low temperature shift catalysts and some CO2 removal systems are sensitive to sulfur and it may be necessary to include a
desulphurization step during the start-up of some HTS catalysts. The level of residual sulfur is so low in VSG-F101, that no special desulphurization step is usually
needed. Reduction and start-up In plants based on steam reforming of hydrocarbons no separate reduction procedure is required for the HTS catalyst as the
introduction of process gas serves to activate, desulfurize and commission the catalyst bed. It is therefore convenient to bring the catalyst on-line as follows: 1 Purge
the reactor free of air with an inert gas and heat the catalyst above the condensation temperature at a rate of about 50o C (90o F) per hour. 2 Care should be taken to
ensure that the catalyst is not dried excessively prior to reduction. This can occur if the catalyst is held in hot nitrogen circulation for an excessive period (24 hrs+),
for example if there are problems elsewhere in the plant during start-up. When wet process gas is introduced to the dried oxidized catalyst, structural changes that
are exothermic can be initiated, leading to temperatures in excess of 450o C (840o F). To avoid this phenomenon, introduce process gas as soon as possible after the
catalyst is hot enough, or suspend nitrogen circulation whilst problems elsewhere are attended to once the bed is up to temperature. Should an exotherm occur when
process gas is admitted, continue introducing feed to remove the heat generated, and keep the vessel at low pressure. If excessive drying is suspected, it is possible
to rehydrate the catalyst by controlled addition of steam, obviously monitoring temperatures carefully whilst small amounts of steam are introduced.
14. 14. Refinery Process Stream Purification Refinery Process Catalysts Troubleshooting Refinery Process Catalyst Start-Up / Shutdown Activation Reduction In-situ
Ex-situ Sulfiding Specializing in Refinery Process Catalyst Performance Evaluation Heat & Mass Balance Analysis Catalyst Remaining Life Determination
Catalyst Deactivation Assessment Catalyst Performance Characterization Refining & Gas Processing & Petrochemical Industries Catalysts / Process Technology -
Hydrogen Catalysts / Process Technology – Ammonia Catalyst Process Technology - Methanol Catalysts / process Technology – Petrochemicals Specializing in the
Development & Commercialization of New Technology in the Refining & Petrochemical Industries Web Site: www.GBHEnterprises.com It should be noted that
this phenomenon only occurs on the initial start up of the HTS catalyst and does not occur on subsequent start-ups. 3 Establish a flow of process gas or steam
through the reactor at a wet gas space velocity in the range 200-1000 h-1 . Allow any water that does condense on the catalyst to drain from the vessel. VSG-F101
reduction will start at about 150o C (300o F), if hydrogen is present and so process gas can be utilized at an early stage during heating. 4 Increase the catalyst inlet
temperature at a rate of 50o C (90o F) per hour until the bed temperature reaches 300o C (570o F). Reduction will continue gradually until the normal operating
temperature is reached. 5 The high temperature shift reaction will gradually begin at temperatures in the range 300-320o C (570-610o F) and a temperature profile
will develop through the bed. The temperature rise will be about 13.5o C (24o F) for every 1% of carbon monoxide (in dry process gas) that is converted. It is
important, therefore, to restrict the amount of carbon monoxide and/or the bed inlet temperature to prevent the bed outlet temperature exceeding 500o C (930o F)
during the reduction procedure. 6 If required any residual sulfur in the catalyst will be converted to hydrogen sulfide at bed temperatures in the range 350-400o C
(660-750o F). It is therefore necessary to maintain the catalyst bed at these temperatures for a period long enough for the sulfur to be completely reduced. Bed inlet
temperature should be increased to at least 370o C (700o F). VSG-F101 contains less than 0.025% w/w sulfur and the desulphurization period should be only about
4 hours from the first introduction of process gas. It is usual to bring the catalyst on line without the need for a special desulphurization step. It may be prudent to
check the sulfur content in the outlet stream before bringing the LTS on-line. 7 Increase the process gas rates and adjust the bed inlet temperature to the start of run
operating value. The above procedure is chosen as a reasonable compromise between energy use and stress on the plant equipment. It should be used during the first
reduction of a new catalyst in order to avoid condensation on the catalyst, which can leach any soluble chromium (Vl) from the catalyst, weakening its structure and
reducing its life. During subsequent start-ups, plant equipment permitting, steam or normal process gas can be used to warm up the catalyst from cold, and heating
rates of 100-150o C/h (180-270o F/h) can be employed without any detrimental effect to the catalyst.
15. 15. Refinery Process Stream Purification Refinery Process Catalysts Troubleshooting Refinery Process Catalyst Start-Up / Shutdown Activation Reduction In-situ
Ex-situ Sulfiding Specializing in Refinery Process Catalyst Performance Evaluation Heat & Mass Balance Analysis Catalyst Remaining Life Determination
Catalyst Deactivation Assessment Catalyst Performance Characterization Refining & Gas Processing & Petrochemical Industries Catalysts / Process Technology -
Hydrogen Catalysts / Process Technology – Ammonia Catalyst Process Technology - Methanol Catalysts / process Technology – Petrochemicals Specializing in the
Development & Commercialization of New Technology in the Refining & Petrochemical Industries Web Site: www.GBHEnterprises.com Greater care must be
taken if the catalyst has been wetted during the shut-down, and in this case the catalyst must be warmed up slowly at first to allow the pellets to dry out. Once this
has been achieved, heating rates can be increased to 100- 150o C/h (180-270o F/h). Operation of VULCAN Series VSG-F101 Plants based on steam reforming
usually incorporate an HTS stage followed either by a PSA unit or a LTS, CO2 removal and methanation stages. Whatever the plant design, it is usual to operate the
HTS catalyst to give maximum carbon monoxide conversion. In plants with more than one shift reactor, a more flexible operation is possible and bed temperatures
must be carefully optimized. Optimum conditions can usually be determined by trial and error. When requested, GBH Enterprises, Ltd., Catalyst Process
Technology will give advice based on calculations using its own specialized computer programs. The HTS reactor is integrated with the process heat recovery
system. It is usually preceded by, and in many modern plants also followed by, a waste heat boiler. The flexibility of the HTS inlet temperature can therefore be
limited by steam requirements and boiler performance so that operation under optimum conditions will not always be possible. The normal life of HTS catalysts in
ammonia and hydrogen plants is 3-5 years although in some cases it can be longer. End of life may be indicated by an increase in carbon monoxide slip and the end
of the temperature profile moving towards and through the end of the bed. It is normal practice, at the start of life, to take advantage of the high initial activity of
these catalysts by running at a low inlet temperature (around 300o C/570o F), although in some cases this cannot be achieved due to limitations with the upstream or
downstream heat recovery requirements. As the catalyst ages and loses activity over its operational life, it is necessary to raise the inlet temperature gradually to
maintain the minimum CO slip, which corresponds to the maximum CO conversion and maximum temperature rise across the bed. Over the life of the catalyst the
inlet temperature would typically rise 30-40o C (54-72o F) depending on the initial inlet bed temperature. Catalyst operating life may also be shortened as a result
of high pressure drop caused by the accumulation of deposits on the top of the catalyst bed. Depending upon the position of the deposits in the bed, it is sometimes
possible to remove these deposits by using a vacuum device during a convenient plant shut-down.
16. 16. Refinery Process Stream Purification Refinery Process Catalysts Troubleshooting Refinery Process Catalyst Start-Up / Shutdown Activation Reduction In-situ
Ex-situ Sulfiding Specializing in Refinery Process Catalyst Performance Evaluation Heat & Mass Balance Analysis Catalyst Remaining Life Determination
Catalyst Deactivation Assessment Catalyst Performance Characterization Refining & Gas Processing & Petrochemical Industries Catalysts / Process Technology -
Hydrogen Catalysts / Process Technology – Ammonia Catalyst Process Technology - Methanol Catalysts / process Technology – Petrochemicals Specializing in the
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 32/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
Development & Commercialization of New Technology in the Refining & Petrochemical Industries Web Site: www.GBHEnterprises.com If the deposits are lying
in the top section of the bed then this technique can be very effective, and an extension of the operating life may be achieved. If the deposits have migrated down
into the main body of the bed, then vacuuming will be of limited use. Loss of activity under normal conditions is usually caused by slow thermal sintering, in which
the small magnetite crystals agglomerate together in spite of the stabilizing effect of the chromia. The larger magnetite crystals have a lower active surface area, and
hence the catalyst activity decreases. The higher the temperature the greater the rate of sintering. In addition, the effects of certain poisons such as silica can reduce
catalyst activity and life. Temperature profile Performance of the catalyst may be monitored during operation by the slope of the temperature profile together with
the corresponding increase of outlet carbon monoxide concentration towards the end of life. The temperature profile should not move down the bed unless there are
unusual problems. These may be deposition of solids such as soda, silica, potash etc from upstream equipment (such as a waste heat boiler leak or high silica
refractory), which block the bed and interfere with gas flow. The most common symptom of blockage is increasing pressure drop. Common problems can usually be
identified from routine measurement of bed temperatures, pressure drop through the bed and analysis of outlet carbon monoxide concentration. Advice should be
requested from GBH Enterprises as soon as any unusual conditions are experienced. Deposition of solids in the catalyst bed If any solids are deposited on the top of
the catalyst bed causing increased pressure drop they should be removed. It is then possible to purge the reactor with inert gas and vacuum extract any contaminated
catalyst together with the deposit from the top of the bed. Caution: great care should be taken and procedures well defined before a person enters a vessel containing
an inert atmosphere. Depending on the quantity of catalyst that has been contaminated by the deposit it may be necessary to replace with an equivalent volume of
new catalyst. No special reduction procedure will be required for the new catalyst.
17. 17. Refinery Process Stream Purification Refinery Process Catalysts Troubleshooting Refinery Process Catalyst Start-Up / Shutdown Activation Reduction In-situ
Ex-situ Sulfiding Specializing in Refinery Process Catalyst Performance Evaluation Heat & Mass Balance Analysis Catalyst Remaining Life Determination
Catalyst Deactivation Assessment Catalyst Performance Characterization Refining & Gas Processing & Petrochemical Industries Catalysts / Process Technology -
Hydrogen Catalysts / Process Technology – Ammonia Catalyst Process Technology - Methanol Catalysts / process Technology – Petrochemicals Specializing in the
Development & Commercialization of New Technology in the Refining & Petrochemical Industries Web Site: www.GBHEnterprises.com Sulfur During use the
catalyst will establish an equilibrium with any sulfur that is present in the inlet gas. Any unexpected sulfur entering the catalyst vessel will be retained by the
catalyst as iron sulfide and then slowly released as normal conditions are resumed. In steam reforming flowsheets the inlet sulfur level should be much less than 1
ppm. However, a HTS catalyst may be used downstream of coal-based or partial oxidation units where the sulfur levels may be significantly higher. For
concentrations of sulfur compounds less than 200 ppm in the inlet gas there should generally be no significant effect on the catalyst. Above this level bulk FeS will
be formed which has only about half the activity of magnetite and allowance for this must be made in the initial design calculations. Frequent cycling between
sulfiding and non-sulfiding conditions should be avoided although the catalyst is strong enough to withstand occasional cycling during plant mal-operation. GBH
Enterprises can also offer VULCAN Series VIG SGS201/202/203, a cobalt molybdenum catalyst, which has been developed for shift conversion in a high sulfur
environment. Details are available from GBH Enterprises, Ltd. Catalyst Process Technology’s web site, at www.gbhenterprises.com . Shut-down During a short
shut-down VSG-F101 may be left in an atmosphere of process gas or steam at operating pressure and temperature. This can result in a partial oxidation of the
catalyst that will be reduced rapidly during restart. If the vessel is likely to cool during the shut-down period it should be purged with an inert gas to prevent
condensation of water. In addition the vessel drains should be checked and any accumulation of condensate within the vessel drained off.
18. 18. Refinery Process Stream Purification Refinery Process Catalysts Troubleshooting Refinery Process Catalyst Start-Up / Shutdown Activation Reduction In-situ
Ex-situ Sulfiding Specializing in Refinery Process Catalyst Performance Evaluation Heat & Mass Balance Analysis Catalyst Remaining Life Determination
Catalyst Deactivation Assessment Catalyst Performance Characterization Refining & Gas Processing & Petrochemical Industries Catalysts / Process Technology -
Hydrogen Catalysts / Process Technology – Ammonia Catalyst Process Technology - Methanol Catalysts / process Technology – Petrochemicals Specializing in the
Development & Commercialization of New Technology in the Refining & Petrochemical Industries Web Site: www.GBHEnterprises.com Reduction and start-up of
VULCAN VSG-C111 catalysts LTS catalysts must be reduced with hydrogen before use. This procedure converts the stable copper oxide component of the new
catalyst into reactive copper metal. During reduction and operation both the zinc oxide and alumina components are unchanged and act as a support, which
stabilizes the copper metal crystallites and as a reservoir for poisons. CuO + H2 → Cu + H2O ΔH = -81 kJ/mol Since the reaction is exothermic, the reduction
generates large quantities of heat and depends on having equipment available to pass diluent inert gas through the LTS reactor. The easiest procedure is to pass a
continuous stream of inert gas, usually methane or nitrogen, through the catalyst bed on a “once through” basis. Although this method can be relatively expensive it
has the advantage of allowing a high space velocity during reduction, which will complete the procedure in about 12-24 hours. The alternative procedure is to
recycle inert gas, usually nitrogen, through the catalyst bed via a special reduction loop, which also includes a recycle compressor and start-up heater. Space
velocity will be limited by the capacity of the recycle compressor but should preferably be at least 300 h- 1 Care should be taken to ensure that the inert carrier gas
is free from reducing components (such as hydrogen or CO) and oxidizing components (oxygen). In the event that natural gas is used as the inert carrier the quantity
of heavier hydrocarbons should be minimized as such hydrocarbons can crack over copper catalysts. The carrier gas should also be free of catalyst poisons such as
sulfur or chloride. With recycle systems there are several important points to remember 1 If the reformer is being used as the start-up heater, then carbon dioxide,
evolved from residual carbonates in the LTS catalyst, may methanate and the product methane can crack on the nickel based reforming catalyst in the reformer and
thereby deposit carbon. There are various procedures to prevent this from happening and GBH Enterprises, Ltd. Catalyst Process Technology can provide
recommendations if required. 2 The concentration of hydrogen entering the LTS catalyst bed should not exceed 0.5% v/v during the early stages of reduction in
order to limit the temperature rise if unreacted hydrogen builds up in the recycle loop.
19. 19. Refinery Process Stream Purification Refinery Process Catalysts Troubleshooting Refinery Process Catalyst Start-Up / Shutdown Activation Reduction In-situ
Ex-situ Sulfiding Specializing in Refinery Process Catalyst Performance Evaluation Heat & Mass Balance Analysis Catalyst Remaining Life Determination
Catalyst Deactivation Assessment Catalyst Performance Characterization Refining & Gas Processing & Petrochemical Industries Catalysts / Process Technology -
Hydrogen Catalysts / Process Technology – Ammonia Catalyst Process Technology - Methanol Catalysts / process Technology – Petrochemicals Specializing in the
Development & Commercialization of New Technology in the Refining & Petrochemical Industries Web Site: www.GBHEnterprises.com 3 In some cases the
“minimum gas density limit” of the compressor may restrict the maximum hydrogen concentration in recycle gas during the final stages of reduction. 4 Water
evolved from the catalyst during reduction must be removed from the closed recycle loop and not be recycled through the catalyst bed. 5 Hydrogen and nitrogen
streams need to be free from water and oxygen that will interfere with the reduction. Nitrogen should be free of hydrogen as this can lead to excess hydrogen being
fed to the catalyst. Reduction procedure The following reduction procedure is recommended for use in plants with facilities for either “once-through” or “circulating
recycle” systems for catalyst reduction. 1 Purge the reactor with inert gas until all oxygen has been removed. Establish a flow of inert gas and heat the catalyst bed
to 120o C (250o F) at a rate of 50o C (90o F) per hour or as governed by the mechanical design of the equipment. Any convenient pressure, up to operating
pressure, may be chosen for the catalyst reduction. In a circulating system a high pressure is normally preferred as it allows a higher gas flow to be achieved in the
system, and the higher partial pressure of hydrogen helps the reduction. 2 Increase the inert gas flow rate to the maximum space velocity possible. Ensure that both
the hydrogen flow meter and analyzer are operating satisfactorily as the temperature approaches 130o C (265o F). Continue heating the catalyst until the top of the
bed is at 180o C (355o F). The temperature of the inert gas should not exceed 210o C (410o F) during the initial heating. If the inert gas space velocity is less than
300 h-1 more care is necessary as there can be poor gas distribution that can lead to localized overheating. Start recording bed temperatures during warm-up to
confirm that the thermocouples are responding correctly and that the gas is well distributed through the bed. 3 When at least the top third of the catalyst bed has
reached 160o C (320o F) hydrogen should be introduced into the carrier gas entering the bed up to a maximum of 1.0% v/v. Once the reduction reaction has started
it will be necessary to record the temperature at different points in the catalyst bed to determine the progress of the temperature profile at regular time
20. 20. Refinery Process Stream Purification Refinery Process Catalysts Troubleshooting Refinery Process Catalyst Start-Up / Shutdown Activation Reduction In-situ
Ex-situ Sulfiding Specializing in Refinery Process Catalyst Performance Evaluation Heat & Mass Balance Analysis Catalyst Remaining Life Determination
Catalyst Deactivation Assessment Catalyst Performance Characterization Refining & Gas Processing & Petrochemical Industries Catalysts / Process Technology -
Hydrogen Catalysts / Process Technology – Ammonia Catalyst Process Technology - Methanol Catalysts / process Technology – Petrochemicals Specializing in the
Development & Commercialization of New Technology in the Refining & Petrochemical Industries Web Site: www.GBHEnterprises.com intervals. If the reduction
reaction is slow with a bed inlet temperature of 180o C (355o F) then the inlet temperature should be raised cautiously to 190-200o C (375-390o F) and held steady
at the temperature which gives a satisfactory reduction rate. 4 Once reduction has started and a steady temperature profile has been established, the hydrogen
concentration should be increased. With nitrogen as carrier gas the hydrogen concentration can be increased to 1.5% v/v and with natural gas as carrier gas the
hydrogen concentration may be increased to 2.0-2.5% v/v. The peak temperature in the bed should not, however, exceed 230o C (445o F) and the hydrogen
concentration should be changed as necessary to control the temperature rise and thereby limit the peak bed temperature. Once reduction has started it may be
possible to decrease the temperature of inlet gas entering the catalyst bed to 180o C (355o F) or less. The temperature rise for 1% hydrogen is typically 30o C (54o
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 33/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
F) in nitrogen and 20o C (36o F) in natural gas. 5 As the reduction proceeds, the temperature profile will move down the catalyst bed. The temperature rise will
decrease when most of the copper oxide has been converted to copper. At this point the catalyst bed inlet temperature may be raised to 200o C (390o F). The inlet
hydrogen concentration can also be increased to 3-5% v/v provided that the maximum temperature limit of 230o C (445o F) in the catalyst bed is not exceeded. 6
When the catalyst reduction appears to be complete the catalyst bed inlet temperature should be raised to 225-230o C (435-445o F) and then if possible, the inlet
hydrogen concentration in the inert gas should also be increased to 20% v/v. This procedure should take not less than two hours. No temperature rise should be
observed and the maximum catalyst temperature should not exceed 230o C (445o F). Analysis should indicate that the hydrogen concentration inlet and exit of the
catalyst bed are within 0.2% of each other. 7 The catalyst reduction is complete and the reactor should be commissioned.
21. 21. Refinery Process Stream Purification Refinery Process Catalysts Troubleshooting Refinery Process Catalyst Start-Up / Shutdown Activation Reduction In-situ
Ex-situ Sulfiding Specializing in Refinery Process Catalyst Performance Evaluation Heat & Mass Balance Analysis Catalyst Remaining Life Determination
Catalyst Deactivation Assessment Catalyst Performance Characterization Refining & Gas Processing & Petrochemical Industries Catalysts / Process Technology -
Hydrogen Catalysts / Process Technology – Ammonia Catalyst Process Technology - Methanol Catalysts / process Technology – Petrochemicals Specializing in the
Development & Commercialization of New Technology in the Refining & Petrochemical Industries Web Site: www.GBHEnterprises.com Controlling the catalyst
reduction The reduction procedure has been designed to limit the temperature rise in the catalyst bed by restricting the hydrogen concentration. This ensures that the
maximum temperature in the bed does not exceed 230o C (445o F) and the maximum catalyst activity is achieved. The reduction reaction is indicated by the
temperature profile which moves from the inlet to exit of the catalyst bed at a rate which depends on inert gas space velocity, hydrogen concentration and bed inlet
temperature. During the whole of the reduction period it is important that operators should determine the inlet and exit hydrogen concentration at regular intervals.
The difference between these two measurements during the time of the reduction represents the volume of hydrogen consumed. Any oxygen present in carrier gas
will also react with hydrogen to form water. Normally the volume of hydrogen required for the reduction is 185 Nm3 /m3 (195 scf/ft3 ) for VULCAN Series VSG
C111 catalysts. A comparison of the hydrogen consumed against the theoretical consumption should be made as a cross check against the progress of the reduction.
The volume of water forming during the reduction procedure will also provide an indication of the progress. Measurement of water produced should only be used as
a rough check on hydrogen uptake. VULCAN Series VSG C111 catalysts will produce 240 kg water/m3 (15 lb water/ft3 ) catalyst, from the reduction process.
Water formed from oxygen present in the inert gas should not be included in any estimate. Again this can be used as a cross check against the progress of the
reduction. Catalyst reduction is virtually completed when the inlet and outlet hydrogen concentrations are the same and the whole bed is above a temperature of
225o C (435o F). The volume of hydrogen consumed should confirm this. It may be difficult to achieve exactly equal hydrogen concentrations at inlet and outlet of
the bed and reduction may be considered complete when the difference between the two measurements has been less than 0.5% v/v for more than four hours. Any
complex copper-zinc basic carbonates present in the catalyst decompose during reduction and release carbon dioxide. Carbon dioxide can be purged from the
recycle system but if for any reason the catalyst reduction procedure is halted, or the catalyst bed isolated at reduction temperature, then any further carbon dioxide
evolution will lead to an increase in reactor pressure. Pressure should therefore be monitored during the time that a reactor is isolated, when it contains partially or
freshly reduced catalyst, and any increase in pressure controlled by venting.
22. 22. Refinery Process Stream Purification Refinery Process Catalysts Troubleshooting Refinery Process Catalyst Start-Up / Shutdown Activation Reduction In-situ
Ex-situ Sulfiding Specializing in Refinery Process Catalyst Performance Evaluation Heat & Mass Balance Analysis Catalyst Remaining Life Determination
Catalyst Deactivation Assessment Catalyst Performance Characterization Refining & Gas Processing & Petrochemical Industries Catalysts / Process Technology -
Hydrogen Catalysts / Process Technology – Ammonia Catalyst Process Technology - Methanol Catalysts / process Technology – Petrochemicals Specializing in the
Development & Commercialization of New Technology in the Refining & Petrochemical Industries Web Site: www.GBHEnterprises.com In addition, if the reactor
is to remain isolated for any length of time after the reduction is completed but before it is commissioned, catalyst bed temperatures should be monitored frequently.
If any increase in temperature is detected the reactor should be immediately purged with inert gas to avoid any rapid temperature rise. Hydrogen source Almost any
gas containing hydrogen is suitable for the reduction e.g. methanator gas, carbon dioxide removal or high temperature shift reactor effluent gas. Hydrogen should be
free of sulfur or chlorine and, if any carbon monoxide is present, allowance should be made for the extra temperature rise during reduction. Natural gas Natural gas
is used as the inert carrier gas during reduction in many natural gas/steam reforming plants. Any high molecular weight hydrocarbons in the natural gas can crack in
the pre-heater at temperatures below 300o C (570o F) to produce hydrogen. Most types of natural gas have been safely used at a maximum catalyst temperature of
230o C (445o F) so it is recommended that care should be taken in measuring the hydrogen concentration carefully at the catalyst bed inlet and that the bed
temperature be carefully controlled. Start-up If the catalyst has already been reduced but is cold, the bed should be warmed to a temperature above the dew point
with inert gas before process gas is introduced to the reactor. When process gas first contacts the catalyst the bed temperatures will usually increase rapidly as the
reaction comes to equilibrium with process conditions. The peak temperature may reach 260o C (500o F) or higher at this stage but there will be no damage to the
catalyst because the peak will quickly pass through the bed. The high temperature can be moved quickly through the bed by increasing the flow of process gas to
design rates as soon as possible. The catalyst bed inlet temperature should also be held as low as possible provided that it is at least 20o C (35o F) above the dew
point. For most duties this corresponds to an inlet temperature of about 200o C (390o F). If there are particular reasons for avoiding a temperature peak there are
several ways by which it can be minimized.
23. 23. Refinery Process Stream Purification Refinery Process Catalysts Troubleshooting Refinery Process Catalyst Start-Up / Shutdown Activation Reduction In-situ
Ex-situ Sulfiding Specializing in Refinery Process Catalyst Performance Evaluation Heat & Mass Balance Analysis Catalyst Remaining Life Determination
Catalyst Deactivation Assessment Catalyst Performance Characterization Refining & Gas Processing & Petrochemical Industries Catalysts / Process Technology -
Hydrogen Catalysts / Process Technology – Ammonia Catalyst Process Technology - Methanol Catalysts / process Technology – Petrochemicals Specializing in the
Development & Commercialization of New Technology in the Refining & Petrochemical Industries Web Site: www.GBHEnterprises.com 1 By increasing reactor
pressure to design level with inert gas before introducing process gas. 2 Introducing process gas at low pressure while venting gas at the reactor exit. This is
particularly easy after reducing catalyst with a ‘once-through’ flow of natural gas by gradually replacing the flow of natural gas by process gas and then opening the
inlet and exit valves fully while closing the vent to commission the reactor.
24. 24. Refinery Process Stream Purification Refinery Process Catalysts Troubleshooting Refinery Process Catalyst Start-Up / Shutdown Activation Reduction In-situ
Ex-situ Sulfiding Specializing in Refinery Process Catalyst Performance Evaluation Heat & Mass Balance Analysis Catalyst Remaining Life Determination
Catalyst Deactivation Assessment Catalyst Performance Characterization Refining & Gas Processing & Petrochemical Industries Catalysts / Process Technology -
Hydrogen Catalysts / Process Technology – Ammonia Catalyst Process Technology - Methanol Catalysts / process Technology – Petrochemicals Specializing in the
Development & Commercialization of New Technology in the Refining & Petrochemical Industries Web Site: www.GBHEnterprises.com Operation of VULCAN
Series VSG-C111 catalysts It is important to operate the LTS catalyst under optimum conditions to achieve the potential savings in plant costs. The LTS catalyst is
sensitive to changes in operating conditions but it is not difficult to maintain fixed steam ratio, pressure and gas composition so that the only real variable is the
catalyst inlet temperature. During the commissioning procedure the bed inlet temperature is gradually increased until the carbon monoxide concentration in exit gas
falls to the minimum level for the conditions. This is the optimum level for maximum CO conversion and at higher inlet temperatures the carbon monoxide level
will again increase. As the catalyst ages or is poisoned it will be necessary to increase the inlet temperature to maintain the minimum carbon monoxide
concentration in the exit gas. LTS catalysts often operate close to condensation conditions during the early part of the catalyst life. To avoid condensation of water
either in the catalyst pores or onto the bed the inlet temperature should be at least 20o C (35o F) above the dew point at all times. This may mean that operation will
be at temperatures higher than the optimum until catalyst activity has fallen sufficiently for the actual and optimum operating temperatures to correspond. This is
not a problem because at temperatures in the range 200-205o C (390-400o F) the difference between the equilibrium outlet carbon monoxide concentration and the
optimum will be very small and the actual outlet concentration will remain constant for a long period. During the normal operating life of the catalyst, optimum
operating conditions can be maintained by a gradual increase of the bed inlet temperature as soon as the carbon monoxide level increases slightly. Whenever
changes in steam ratio or gas composition occur the bed inlet should be checked to ensure that it is still at the optimum level. This should be done by increasing or
decreasing the bed inlet temperature by 5o C (10o F) and then checking the carbon monoxide concentration at the bed outlet when conditions have stabilized. If a
decrease in the carbon monoxide concentration is detected the procedure is repeated until the minimum level has been reached. A simple way of determining CO
slip is to observe the methanator temperature rise if the flowsheet features this reactor. Minimum CO slip from the low temperature shift will correspond to the
minimum temperature rise across the methanator. Towards the end of the catalyst life the bed exit temperature will often reach the design level, which might
occasionally correspond to the specified maximum operating temperature of 250o C (480o F). This is however a conservative figure and operation up to at least
270o C (520o F) will still be possible.
25. 25. Refinery Process Stream Purification Refinery Process Catalysts Troubleshooting Refinery Process Catalyst Start-Up / Shutdown Activation Reduction In-situ
Ex-situ Sulfiding Specializing in Refinery Process Catalyst Performance Evaluation Heat & Mass Balance Analysis Catalyst Remaining Life Determination
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 34/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
Catalyst Deactivation Assessment Catalyst Performance Characterization Refining & Gas Processing & Petrochemical Industries Catalysts / Process Technology -
Hydrogen Catalysts / Process Technology – Ammonia Catalyst Process Technology - Methanol Catalysts / process Technology – Petrochemicals Specializing in the
Development & Commercialization of New Technology in the Refining & Petrochemical Industries Web Site: www.GBHEnterprises.com At higher temperatures
however the deactivation rate for partially poisoned catalyst is faster and the carbon monoxide equilibrium level becomes increasingly unfavorable. Operation with
high outlet carbon monoxide concentrations will become increasingly expensive. It is usually more economic to plan a catalyst change before the performance
deteriorates beyond the design level. By-product formation Methanol and, to a lesser extent amines formed from methanol produced in the LTS converter and any
nitrogen compounds inlet the converter (such as ammonia formed in the secondary reformer), are formed in low temperature shift catalyst beds, particularly in the
early stages of life when catalyst activity is at its maximum. By-product formation is very sensitive to temperature and can be minimized by running with a low inlet
temperature. This is consistent with maximizing CO conversion. As ageing occurs, by-product formation is reduced. If operators require ultra-low methanol by-
product formation, then GBH Enterprises, Ltd. Catalyst Process Technology should be consulted. Temperature profile The temperature profile through the catalyst
bed is a useful indicator to follow changes in catalyst activity especially when the outlet carbon monoxide concentration is at the equilibrium level. For a fresh
catalyst most of the reaction and the corresponding temperature rise will be at the top of the bed. Loss of catalyst activity (or catalyst deactivation) during operation
is largely due to poisoning. Because the catalysts are “self-guarding” poisons accumulate at the top of the catalyst bed. The temperature profile will therefore
gradually move from the inlet towards the exit of the catalyst bed as more poisons are absorbed. Towards the end of the catalyst life when the reaction zone has
reached the bottom of the bed and the outlet carbon monoxide level has started to increase from the equilibrium concentration, the catalyst should be changed. Any
variation from a typical temperature profile will indicate abnormal conditions. 1 A slow increase in bed temperature giving a flatter than average profile can indicate
that the whole catalyst bed has been partially deactivated. This may be due to the presence of liquid water in the bed that would block the catalyst pores and wash
poisons from the top of the catalyst down to the middle or bottom levels. The catalyst may also have been overheated.
26. 26. Refinery Process Stream Purification Refinery Process Catalysts Troubleshooting Refinery Process Catalyst Start-Up / Shutdown Activation Reduction In-situ
Ex-situ Sulfiding Specializing in Refinery Process Catalyst Performance Evaluation Heat & Mass Balance Analysis Catalyst Remaining Life Determination
Catalyst Deactivation Assessment Catalyst Performance Characterization Refining & Gas Processing & Petrochemical Industries Catalysts / Process Technology -
Hydrogen Catalysts / Process Technology – Ammonia Catalyst Process Technology - Methanol Catalysts / process Technology – Petrochemicals Specializing in the
Development & Commercialization of New Technology in the Refining & Petrochemical Industries Web Site: www.GBHEnterprises.com 3 If the temperature
profile appears to be normal but the outlet carbon monoxide is higher than expected then gas may be bypassing part of the catalyst bed. Steam The use of steam
alone should be avoided as far as possible to prevent condensation of water in the catalyst bed. During plant upsets, short periods of steaming may be unavoidable
but it is far better to isolate the low temperature shift reactor and reduce pressure to depress the dew point. The reactor should then be purged with an inert gas.
Shut-down During an extended plant shut-down, when the reactor can cool down, process gas must be purged from the reactor to avoid the condensation of water
on to the catalyst. This could damage the catalyst by washing poisons from the top to the bottom part of the catalyst bed onto fresh unpoisoned catalyst lower down
the bed. Pressure should therefore be decreased to atmospheric, before the temperature falls below the dew point, and the vessel purged with an inert gas to remove
all steam. Catalyst poisons Sulfur and chloride are the most serious poisons for LTS catalysts. Of the two, chlorides are the more virulent; however, sulfur tends to
be present in greater concentrations in the process gas and therefore often determines the catalyst life. Chlorine compounds are often present in process gas streams
in extremely small concentrations that cannot be detected by typical analytical procedures. The poisoning effect is cumulative so that any concentration of chlorine
in process gas will eventually poison the catalyst bed and detection is only possible by the analysis of samples then from discharged catalyst. The formulation of
GBH Enterprises, VULCAN Series catalysts to provide thermally stable structures also enhances the ability of these catalysts to absorb poisons. VSG-C111 series
catalysts can absorb chlorides at the top of the bed and guard active catalyst in lower layers, and so extend operating time.
27. 27. Refinery Process Stream Purification Refinery Process Catalysts Troubleshooting Refinery Process Catalyst Start-Up / Shutdown Activation Reduction In-situ
Ex-situ Sulfiding Specializing in Refinery Process Catalyst Performance Evaluation Heat & Mass Balance Analysis Catalyst Remaining Life Determination
Catalyst Deactivation Assessment Catalyst Performance Characterization Refining & Gas Processing & Petrochemical Industries Catalysts / Process Technology -
Hydrogen Catalysts / Process Technology – Ammonia Catalyst Process Technology - Methanol Catalysts / process Technology – Petrochemicals Specializing in the
Development & Commercialization of New Technology in the Refining & Petrochemical Industries Web Site: www.GBHEnterprises.com Strict attention is
necessary however to maintain steam purity and to avoid contamination of feedstocks or process air by chlorine compounds. Solvents containing chlorine should
not be used for cleaning any items of plant equipment. If chloride poisoning is an issue then GBH Enterprises, Ltd. Catalyst Process Technology should be
consulted. Sulfur compounds also affect the operation of VSG-C111 series catalysts but are much less virulent poisons than chlorine compounds. GBH Enterprises,
Ltd. VULCAN Series catalysts are self-guarding against sulfur compounds provided that the typical levels found in ammonia or hydrogen plants based on steam
reforming are not exceeded for long periods. Silica is also present in most process gas streams and is absorbed by the catalyst bed and gradually deactivates the
catalyst. Small amounts of silica are deposited on the catalyst surface but larger quantities react with the catalyst to form zinc silicate. Silica is not a typical catalyst
poison but has the effect of decreasing the catalyst’s capacity for other poisons and therefore allows chlorine and sulfur to pass further into the catalyst bed.
Hydrogen and ammonia plants should always be designed to include sufficient catalyst volume to operate satisfactorily with average levels of poisons present in
feedstocks. Adjustments can be made when increased levels of poisons are detected either by using extra catalyst volume or by installing appropriate guard beds.
28. 28. Refinery Process Stream Purification Refinery Process Catalysts Troubleshooting Refinery Process Catalyst Start-Up / Shutdown Activation Reduction In-situ
Ex-situ Sulfiding Specializing in Refinery Process Catalyst Performance Evaluation Heat & Mass Balance Analysis Catalyst Remaining Life Determination
Catalyst Deactivation Assessment Catalyst Performance Characterization Refining & Gas Processing & Petrochemical Industries Catalysts / Process Technology -
Hydrogen Catalysts / Process Technology – Ammonia Catalyst Process Technology - Methanol Catalysts / process Technology – Petrochemicals Specializing in the
Development & Commercialization of New Technology in the Refining & Petrochemical Industries Web Site: www.GBHEnterprises.com
Recommended
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 35/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 36/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 37/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
(HTS) High Temperature Shift Catalyst (VSG-F101) - Comprehensiev Overview
Gerard B. Hawkins
English
Español
Português
Français
Deutsch
About
Dev & API
Blog
Terms
Privacy
Copyright
Support
Share Clipboard
Facebook
Twitter
LinkedIn
Link
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 38/39
9/30/2019 Shift Conversion Catalysts - Operating Manual
Create a clipboard
https://www.slideshare.net/GerardBHawkins/shift-conversion-catalysts-operating-manual 39/39