This document summarizes two formulations of a contact and reactive adhesive (CRD). One formulation is for bonding high viscosity materials like wood, metal, and stone to various substrates. It contains Dispercoll polymers and has a high viscosity of over 100,000 cps. The second formulation is for bonding foam materials and can be applied via spray. It contains different Dispercoll polymers and Nanobyk additive and has a lower viscosity of 900 cps. Both formulations provide initial bonding within an hour and full bonding within 24 hours for the high viscosity formulation and 18 hours for the foam formulation.
This document summarizes two formulations of a contact and reactive adhesive (CRD). One formulation is for bonding high viscosity materials like wood, metal, and stone to various substrates. It contains Dispercoll polymers and has a high viscosity of over 100,000 cps. The second formulation is for bonding foam materials and can be applied via spray. It contains different Dispercoll polymers and Nanobyk additive and has a lower viscosity of 900 cps. Both formulations provide initial bonding within an hour and full bonding within 24 hours for the high viscosity formulation and 18 hours for the foam formulation.
This document summarizes two formulations of a contact and reactive adhesive (CRD). One formulation is for bonding high viscosity materials like wood, metal, and stone to various substrates. It contains Dispercoll polymers and has a high viscosity of over 100,000 cps. The second formulation is for bonding foam materials and can be applied via spray. It contains different Dispercoll polymers and Nanobyk additive and has a lower viscosity of 900 cps. Both formulations provide initial bonding within an hour and full bonding within 24 hours for the high viscosity formulation and 18 hours for the foam formulation.
This document summarizes two formulations of a contact and reactive adhesive (CRD). One formulation is for bonding high viscosity materials like wood, metal, and stone to various substrates. It contains Dispercoll polymers and has a high viscosity of over 100,000 cps. The second formulation is for bonding foam materials and can be applied via spray. It contains different Dispercoll polymers and Nanobyk additive and has a lower viscosity of 900 cps. Both formulations provide initial bonding within an hour and full bonding within 24 hours for the high viscosity formulation and 18 hours for the foam formulation.
Application : High visco for multi substrates & HPL Spray CRD for foam to foam
covestro.com October 19 │ Presentation Title 1
CRD formulation Ingriedients For HPL & multi substrate For foam to foam Dispercoll C 2694/1 69.4 Dispercoll C 84 Dispercoll C 2372/1 37.6 Dispercoll C 74 37.6 Nanobyk 3840 (50% sol) 3.2 S 3030/1 21.5 Revacryl 4522 27.78 Aquaflow NHS 50% Sol Borchigel ALA 2.78 Glycine powder Glycine 3 gr No pH adjustment Total 101.9 99.96 Properties 2 4 NV (% w/w ) 49.13 43.75 Viscosity ( cps ) > 100 000 900 cp/l2/30 rpm pH 9 8 Gramature ( gr/m2 ) 200-250 100 - 150 Application 2 sides by scrapper 2 sides by spray. Flash off time @RT 3' 1 min Initial bonding 1 hr 4' Final bonding 24 hrs 18' Substrates Wood, GRC, Tin plate, Many types of foam & Wood, Al foil,HPL Textile Note HPL & Multi substrates Spray ADH for foam to foam. Storage stability In progress In progress
2 October 19 │ Presentation Title
Application Method
Application is Flash off Press
for 2 sides of (1 minutes at substrates substrate room manually, and temperature for then check for Coating weight spray) initial & final for spray : 100 – bonding 150 gsm (3 – 5 ‘ minutes at room Coating weight temperature for for scrap : 200 – spray) 250 gsm