Professional Documents
Culture Documents
BS en 1926
BS en 1926
1926:2006
12&23<,1*:,7+287%6,3(50,66,21(;&(37$63(50,77('%<&23<5,*+7/$:
BS EN 1926:2006
National foreword
© BSI 2007
ISBN 978-0-580-49936-4
EUROPEAN STANDARD EN 1926
NORME EUROPÉENNE
EUROPÄISCHE NORM December 2006
English Version
Méthodes d'essai des pierres naturelles - Détermination de Prüfverfahren für Naturstein - Bestimmung der einachsigen
la résistance à la compression uniaxiale Druckfestigkeit
CEN members are bound to comply with the CEN/CENELEC Internal Regulations which stipulate the conditions for giving this European
Standard the status of a national standard without any alteration. Up-to-date lists and bibliographical references concerning such national
standards may be obtained on application to the Central Secretariat or to any CEN member.
This European Standard exists in three official versions (English, French, German). A version in any other language made by translation
under the responsibility of a CEN member into its own language and notified to the Central Secretariat has the same status as the official
versions.
CEN members are the national standards bodies of Austria, Belgium, Cyprus, Czech Republic, Denmark, Estonia, Finland, France,
Germany, Greece, Hungary, Iceland, Ireland, Italy, Latvia, Lithuania, Luxembourg, Malta, Netherlands, Norway, Poland, Portugal, Romania,
Slovakia, Slovenia, Spain, Sweden, Switzerland and United Kingdom.
© 2006 CEN All rights of exploitation in any form and by any means reserved Ref. No. EN 1926:2006: E
worldwide for CEN national Members.
EN 1926:2006 (E)
Contents page
Foreword......................................................................................................................................................................3
1 Scope ..............................................................................................................................................................4
2 Normative references ....................................................................................................................................4
3 Principle..........................................................................................................................................................4
4 Terms and Definitions ...................................................................................................................................4
5 Symbols ..........................................................................................................................................................4
6 Apparatus .......................................................................................................................................................5
7 Preparation of specimens.............................................................................................................................5
7.1 Sampling .........................................................................................................................................................5
7.2 Test specimens ..............................................................................................................................................5
7.3 Surface preparation .......................................................................................................................................5
7.3.1 General............................................................................................................................................................5
7.3.2 Capping with mortar ......................................................................................................................................6
7.4 Conditioning of specimen before testing....................................................................................................6
8 Procedure .......................................................................................................................................................6
8.1 Measuring the specimen ...............................................................................................................................6
8.2 Placing the specimen in the testing machine.............................................................................................6
8.3 Loading ...........................................................................................................................................................6
9 Expression of results ....................................................................................................................................6
10 Test report ......................................................................................................................................................7
Annex A (normative) Determination of the compressive strength of armourstone ...........................................9
A.1 Scope ..............................................................................................................................................................9
A.2 Normative references ....................................................................................................................................9
A.3 Principle..........................................................................................................................................................9
A.4 Definitions and symbols ...............................................................................................................................9
A.5 Apparatus .......................................................................................................................................................9
A.6 Preparation of specimens.............................................................................................................................9
A.6.1 Sampling .........................................................................................................................................................9
A.6.2 Test specimens ..............................................................................................................................................9
A.6.3 Surface preparation .....................................................................................................................................10
A.6.4 Conditioning of specimen before testing..................................................................................................10
A.7 Procedure .....................................................................................................................................................10
A.8 Expression of results ..................................................................................................................................10
A.9 Test report ....................................................................................................................................................10
Annex B (informative) Determination of the point load strength index of natural stone.................................12
B.1 General..........................................................................................................................................................12
B.2 Background ..................................................................................................................................................12
B.3 Correlation data ...........................................................................................................................................12
Annex C (normative) Statistical evaluation of the results ...................................................................................13
C.1 Scope ............................................................................................................................................................13
C.2 Symbols and definitions .............................................................................................................................13
C.3 Statistical evaluation of test results ..........................................................................................................14
Annex D (informative) Bibliografy related to Annex B.........................................................................................16
Bibliography ..............................................................................................................................................................17
2
EN 1926:2006 (E)
Foreword
This document (EN 1926:2006) has been prepared by Technical Committee CEN/TC 246 “Natural stones”,
the secretariat of which is held by UNI.
This European Standard shall be given the status of a national standard, either by publication of an identical
text or by endorsement, at the latest by June 2007, and conflicting national standards shall be withdrawn at
the latest by June 2007.
According to the CEN/CENELEC Internal Regulations, the national standards organizations of the following
countries are bound to implement this European Standard: Austria, Belgium, Cyprus, Czech Republic,
Denmark, Estonia, Finland, France, Germany, Greece, Hungary, Iceland, Ireland, Italy, Latvia, Lithuania,
Luxembourg, Malta, Netherlands, Norway, Poland, Portugal, Romania, Slovakia, Slovenia, Spain, Sweden,
Switzerland and United Kingdom.
3
EN 1926:2006 (E)
1 Scope
This European standard specifies a method for determining the uniaxial compressive strength of natural
stones.
2 Normative references
The following referenced documents are indispensable for the application of this document. For dated
references, only the edition cited applies. For undated references, the latest edition of the referenced
document (including any amendments) applies.
EN 197-1, Cement – Part 1: Composition, specifications and conformity criteria for common cements
3 Principle
The specimens, after mechanical preparation of surfaces or, if needed, after capping, are laid and centred on
the plate of a testing machine. A uniformly distributed load is applied and increased continuously until failure
occurs.
5 Symbols
l mean value of the lateral dimension, i.e. the distance between opposite vertical faces of the specimen (if
cubic), in millimetres;
v coefficient of variation.
4
EN 1926:2006 (E)
6 Apparatus
6.1 A surface grinder.
6.3 A test machine of appropriated force, in accordance with EN 12390 and calibrated according to this
standard.
7 Preparation of specimens
7.1 Sampling
The sampling is not the responsibility of the testing laboratory, unless specially requested.
At least 10 specimens are to be tested and the direction of any existing plane of anisotropy recorded.
Test specimens shall be cubes with (70 ± 5) mm or (50 ± 5) mm edges or right circular cylinders whose
diameter and height are equal to (70 ± 5) mm or (50 ± 5) mm.
The lateral dimension or the diameter of the specimen shall be related to the size of the largest grain in the
rock by the ratio of at least 10:1. If the maximum observed dimension of the grains exceeds 7 mm, it is
recommended to have a larger number of specimens in order to obtain representative results.
The axis of the specimen shall be normal to the planes of anisotropy, e.g. bedding planes, foliation, etc. (figure
1a and 2a). If a test with orientation of loading parallel to the planes of anisotropy is required, another set of
specimens with the same dimensional characteristics shall be prepared (Figure 1b and 2b).
7.3.1 General
The faces to which the load is to be applied shall be flat to a tolerance of 0,1 mm in any 100 mm and such that
the top surface lies between two parallel planes which are parallel to the bottom surface, and not greater than
1mm apart for every 100 mm The sides of the specimen shall be smooth and free of abrupt irregularities and
straight to within 0,3 mm over the full length of the specimen.
To meet the above requirements the specimens shall be finished on either a lathe or surface grinder, with final
preparation on a lapping machine if needed.
Capping with mortar according to the procedures indicated in 7.3.2 is to be used only if the indicated
tolerances are not obtainable with the prescribed mechanical preparation. This condition shall be clearly
indicated in the test report.
5
EN 1926:2006 (E)
It is possible to cap the specimen using a mortar made with cement CEM I 52,5 R according to EN 197-1 and
then waiting until the cement has hardened.
Specimens, whether capped or uncapped, shall be dried at (70 ± 5) °C to constant mass. This is assumed to
have been attained when the difference between two weighings at an interval of (24 ± 2) h is not greater than
0,1% of the mass of the specimen. After drying and prior to testing the specimens shall be stored at (20 ±
5) °C until the thermal equilibrium is reached. After that, the tests shall be performed within 24 h.
8 Procedure
The cross-sectional dimensions of the test specimen (lateral dimension for cubic diameter for cylindrical test
specimens) shall be measured to the nearest 0,1 mm by averaging two measures taken at right angles to
each other at about the upper-height and two about the lower-height h of the specimen. The average lateral
dimension l or the average diameter d shall be used for calculating the cross-sectional area. The height of
the specimen shall be determined to the nearest 1,0 mm.
Wipe the bearing surfaces of the testing machine clean and remove any loose grit from the bed faces of the
specimen. Align the specimen carefully with the centre of the ball-seated platen, so that a uniform seating is
obtained. Do not use any packing material.
8.3 Loading
Load on the specimen shall be applied continuously at a constant stress rate of (1 ± 0,5) MPa/s. The
maximum load on the specimen shall be recorded to the nearest 10kN.
9 Expression of results
The uniaxial compressive strength R of each specimen is expressed by the ratio of the failure load of the
specimen and its cross-sectional area before testing, by the equation:
F
R= (1)
A
The result shall be expressed in Megapascals with at least two significant figures. The mean value R shall be
calculated to the nearest 1 MPa.
6
EN 1926:2006 (E)
10 Test report
The test report shall contain the following information:
c) name and address of the testing laboratory and the address where the test was carried out if different
from the testing laboratory;
direction of any existing plane of anisotropy (if relevant to the test), clearly indicated on the sample or on
each specimen by means of two parallel lines;
g) date when the specimens were prepared (if relevant) and the date of testing;
i) dimensions l (or d ) and h in millimetres and the failure load F of each specimen, in kiloNewtons
measured without any decimal place;
k) orientation of the axis of loading with respect to the existing planes of anisotropy;
l) compressive strength R of each specimen, in Megapascals with at least two significant figures;
p) remarks.
The test report shall contain the signature(s) and role(s) of the responsible(s) party(s) for testing and the issue
date of the report. It shall also state that the report shall not be partially reproduced without written consent
from the testing laboratory.
7
EN 1926:2006 (E)
Key
a) load normal to the planes of anisotropy
b) load parallel to the planes of anisotropy
Key
a) load normal to the planes of anisotropy
b) load parallel to the planes of anisotropy
8
EN 1926:2006 (E)
Annex A
(normative)
A.1 Scope
This annex specifies the method for the determination of compressive strength of stones of different size and
irregular shape, which are used in hydraulic protection and regulation structures. The term armourstone is
used for such materials.
A.3 Principle
See clause 3. For materials to be used as armourstone, specimens shall be tested in a condition indicating
their strength in water and in their weakest orientation with respect to any existing plane of anisotropy.
A.5 Apparatus
See clause 6.
A.6.1 Sampling
Each specimen shall be prepared from a separate piece of armourstone. Test specimens shall be cubes with
(50 ± 5) mm edges or right circular cylinders whose diameter and height are equal to (50 ± 5) mm. For the
pieces of armourstone whose compressive strength is lower than or equal to 40 MPa, the use of cubes with
(70 ± 7) mm edges or right circular cylinders whose diameter and heigth are equal to (70 ± 7) mm are allowed.
The lateral dimension or the diameter of the specimen should be related to the size of the largest grain in a
representative piece of the material by a ratio of at least 10:1. For coarse-grained material, cubes or cylinders
having an edge or diameter no greater than 150 mm are admitted. In this case, the maximum dimensions of
the grains shall be indicated in the test report.
9
EN 1926:2006 (E)
The axis of the specimen shall be parallel to the planes of anisotropy, e.g. bedding planes, foliations, etc. If a
test with orientation of loading normal to the anisotropy is required, another set of specimens with the same
dimensional characteristics shall be prepared.
Test specimens shall be fully immersed in tap water at a room temperature of (20 ± 10)°C for (48 ± 4) h and
tested for strength within 1 h of removal from the water, taking care to minimise any changes in moisture
content of the specimen prior to testing.
A.7 Procedure
As in main text, clause 8.
c) name and address of the testing laboratory and the address where the test was carried out if different
from the testing laboratory;
direction of any existing plane of anisotropy (if relevant to the test) to be clearly indicated on the sample
or on each specimen by means of two parallel lines;
10
EN 1926:2006 (E)
g) date when the specimens were prepared (if relevant) and the date of testing;
i) dimensions l (or d ) and h in millimetres and the failure load F of each specimen, in kiloNewtons
measured without any decimal place;
l) compressive strength R of each specimen, in Megapascals with at least two significant figures;
o) description of any specimen breakages that occurred during specimen preparation, detailing the number
of such breakages;
q) remarks.
The test report shall contain the signature(s) and role(s) of the responsible party(ies) for the testing and the
issue date of the report. It shall also state that the report shall not be partially reproduced without the written
consent from the laboratory.
11
EN 1926:2006 (E)
Annex B
(informative)
B.1 General
This informative annex is given to provide a simple method for the factory production control of the uniaxial
compressive strength of natural stone and stone used in hydraulic structures.
B.2 Background
The point load strength index is widely used in rock mechanic applications for obtaining a rapid and cheap
assessment of the variability in rock source strength and is therefore ideal for use in factory production control.
If a correlation for the specific rock type is not available, the general correlation equation given in the
reference in Annex D is as follows:
It is based on an extensive investigation of a wide range of strong and weak rocks. It will not give a very
accurate prediction of compressive strength for all rock types, however, it is recommended as the best
researched single correlation factor to predict the compressive strength of all rock types. An aspect ratio of 2:1
for length to diameter of cylinders is assumed for the compressive strength data in the above correlation
equation.
12
EN 1926:2006 (E)
Annex C
(normative)
C.1 Scope
This annex establishes a method for the statistical treatment of test results obtained following the natural
stone test method described in this standard.
1
x=
n ∑x i
Mean value i
s
Coefficient of variation v= (for individual values)
x
1
x ln =
n ∑ ln x i
Logarithmic Mean i
n −1
( x ln −( k ⋅s ))
Lower expected value E=e s ln where ks (quantile factor) is given in
Table 1
13
EN 1926:2006 (E)
For the calculation of the mean value (x ) , the standard deviation (s) and the coefficient of variation (v), a
normal distribution is assumed.
When calculating the lower expected value (E), a logarithmic normal distribution is assumed. The lower
expected value (E) corresponds to the 5 % quantile of a logarithmic normal distribution for a confidence level
of 75%.
Table C.1 Quantile factor (ks) in dependence on the number of measured values (n) in correspondence
to the 5% quantile for a confidence level of 75%
n ks
3 3,15
4 2,68
5 2,46
6 2,34
7 2,25
8 2,19
9 2,14
10 2,10
15 1,99
20 1,93
30 1,87
40 1,83
50 1,81
8 1,64
14
EN 1926:2006 (E)
EXAMPLE 1 Calculation of mean value, standard deviation, maximum value and minimum value of 6 measured
values:
15
EN 1926:2006 (E)
Annex D
(informative)
The International Society for Rock Mechanics convened a Working Party to produce a ‘Recommended
Suggested Method’ for the determination of the point load strength index. The reference is as follows:
Franklin, J.A. [co-ordinator] (1985), Suggested method for determining Point Load Strength, International
Society for Rock Mechanics Commission on Testing Methods, (revised version). International Journal of Rock
Mechanics, Mining Sciences and Geomechanical Abstracts., Vol 22, pp 51-60.
16
EN 1926:2006 (E)
Bibliography
[1] EN 1925, Natural stone test methods – Determination of water absorption coefficient by capillarity.
[2] EN 1936, Natural stone test methods – Determination of real density and apparent density, and of total
and open porosity.
[3] EN 12370, Natural stone test methods – Determination of resistance to salt crystallisation.
[5] EN 12372, Natural stone test methods – Determination of flexural strength under concentrated load.
[8] EN 13161, Natural stone test methods – Determination of flexural strength under constant moment.
[9] EN 13364, Natural stone test methods – Determination of the breaking load at dowel hole.
[10] EN 13373, Natural stone test methods – Determination of geometric characteristics on units.
[11] EN 13755, Natural stone test methods – Determination of water absorption at atmospheric pressure.
[12] EN 13919, Natural stone test methods - Determination of resistance to ageing by S02 action in the
presence of humidity.
[13] EN 14066, Natural stone test methods – Determination of resistance to ageing by thermal shock.
[14] EN 14146, Natural stone test methods – Determination of the dynamic modulus of elasticity (by
measuring the fundamental resonance frequency).
[15] EN 14147, Natural stone test methods – Determination of resistance to ageing by salt mist.
[18] EN 14231, Natural stone test methods – Determination of the slip resistance by means of the
pendulum tester.
[19] EN 14579, Natural stone test methods – Determination of sound speed propagation.
[20] EN 14580, Natural stone test methods – Determination of static elastic modulus.
[21] EN 14581, Natural stone test methods – Determination of linear thermal expansion coefficient.
[22] EN 14157, Natural stone test methods – Determination of the abrasion resistance.
17
BS EN
1926:2006
BSI — British Standards Institution
BSI is the independent national body responsible for preparing
British Standards. It presents the UK view on standards in Europe and at the
international level. It is incorporated by Royal Charter.
Revisions
British Standards are updated by amendment or revision. Users of
British Standards should make sure that they possess the latest amendments or
editions.
It is the constant aim of BSI to improve the quality of our products and services.
We would be grateful if anyone finding an inaccuracy or ambiguity while using
this British Standard would inform the Secretary of the technical committee
responsible, the identity of which can be found on the inside front cover.
Tel: +44 (0)20 8996 9000. Fax: +44 (0)20 8996 7400.
BSI offers members an individual updating service called PLUS which ensures
that subscribers automatically receive the latest editions of standards.
Buying standards
Orders for all BSI, international and foreign standards publications should be
addressed to Customer Services. Tel: +44 (0)20 8996 9001.
Fax: +44 (0)20 8996 7001. Email: orders@bsi-global.com. Standards are also
available from the BSI website at http://www.bsi-global.com.
In response to orders for international standards, it is BSI policy to supply the
BSI implementation of those that have been published as British Standards,
unless otherwise requested.
Information on standards
BSI provides a wide range of information on national, European and
international standards through its Library and its Technical Help to Exporters
Service. Various BSI electronic information services are also available which give
details on all its products and services. Contact the Information Centre.
Tel: +44 (0)20 8996 7111. Fax: +44 (0)20 8996 7048. Email: info@bsi-global.com.
Subscribing members of BSI are kept up to date with standards developments
and receive substantial discounts on the purchase price of standards. For details
of these and other benefits contact Membership Administration.
Tel: +44 (0)20 8996 7002. Fax: +44 (0)20 8996 7001.
Email: membership@bsi-global.com.
Information regarding online access to British Standards via British Standards
Online can be found at http://www.bsi-global.com/bsonline.
Further information about BSI is available on the BSI website at
http://www.bsi-global.com.
Copyright
Copyright subsists in all BSI publications. BSI also holds the copyright, in the
UK, of the publications of the international standardization bodies. Except as
permitted under the Copyright, Designs and Patents Act 1988 no extract may be
reproduced, stored in a retrieval system or transmitted in any form or by any
means – electronic, photocopying, recording or otherwise – without prior written
permission from BSI.
This does not preclude the free use, in the course of implementing the standard,
of necessary details such as symbols, and size, type or grade designations. If these
details are to be used for any other purpose than implementation then the prior
BSI written permission of BSI must be obtained.
389 Chiswick High Road Details and advice can be obtained from the Copyright & Licensing Manager.
London Tel: +44 (0)20 8996 7070. Fax: +44 (0)20 8996 7553.
Email: copyright@bsi-global.com.
W4 4AL