To cite this article: A. Palanisamy, T. Selvaraj & S. Sivasankaran (2018) Heat treatment effect
on CNC turning of Incoloy 800H superalloy, Materials and Manufacturing Processes, 33:14,
1594-1601, DOI: 10.1080/10426914.2018.1424910
none defined
Table 1. Chemical composition of Incoloy 800H (wt%). Table 2. Tool geometry of uncoated tungsten carbide insert.
C Mo P S Si Cr Ni Ti Al Cu Fe Insert nomenclature Values
0.069 0.76 0.014 0.001 0.13 20.42 31.59 0.57 0.50 0.42 45.562 Clearance angle 5°
Side rake angle 6°
Inclination angle 6°
the capacity of 1300°C and then the rods were water quenched. Major cutting edge angle or approach angle 95°
Included angle or point angle 80°
After solution heat treatment, all the samples were further Nose radius 0.8 mm
heat-treated at 975°C for 60 min using the same heating rate
of 40°C. Then, some samples were cooled in the air called
air-cooled (AC) samples and some samples were cooled in
the furnace itself called furnace-cooled (FC) samples. The
phase diagram and the heat treatment process for the Incoloy
800H superalloys used in the present experimental work as a
schematic are shown in Fig. 1(a). To examine the compressive
strength of the samples under different conditions, the sample
size of 6 mm in diameter with a height of 9 mm (aspect ratio
1.5 as per ASTM E9 standard) was prepared carefully. The
servo-controlled Tinius Olsen H50KL universal testing
machine was used for the compression test at a strain rate of
1 mm/min. During compression test, 30% set height reduction Figure 2. (a) Photograph and tool geometry of cutting insert of CNMA 120408
was used in all the samples. The microstructures of the as- used during turning.
received forged rod, heat-treated samples before compression,
and heat-treated samples after compression were taken using shows the Incoloy 800H rod held in the machine. During
Olympus optical microscope. The appropriate metallographic turning, the length to diameter ratio of 2 (L/D ¼ 50/25) was
procedure was used for the sample preparations. The forma- used in which 50 mm workpiece length was outside of the
tion of titanium carbides, chromium carbides, and fractured chuck, whereas 75 mm workpiece length was inside of the
surfaces were examined using Hitachi S-3000H scanning elec- chuck. The machining length of 40 mm was used to avoid
tron microscope. As-received forged samples and heat-treated undesirable deflection, tool vibration, and chattering.[20] Three
samples were machined using LEADWELL CNC T5 turning samples have been used for each experiment with a new sharp
center under dry environment. The capacity of the machine cutting edge and the average values of the responses were
is 4500 rpm with 7.5 kW power. Figure 1(b) shows the macro- taken for investigation. The turning process was performed
graph of turning experimental setup and the inset of Fig. 1(b) using ISO K20 CNMA 120408-THM (WIDIA-India) uncoated
tungsten carbide tool. Table 2 and Fig. 2 describe the tool
geometry of the insert. In the present investigation, two
important cutting parameters such as cutting speed (35, 45,
and 55 m/min) and the feed rate (0.02, 04, and 0.06 mm/rev)
were varied as mentioned in Table 3, whereas the depth of
cut was maintained by 0.5 mm. Here, according to Special
Metals Corporation, USA, Sandmeyer Steel Company, USA,
and the Incoloy 800 H alloy supplier, tool’s catalog and
previous literature,[21,22] the machining parameters were
selected. Further, lowest levels of cutting speed, feed rate,
and depth of cut were chosen to avoid the undesirable work
deflection, tool vibration, and chattering. In addition, based
on some authors of previous work[23,24] and to have an
improved surface finish, low-level range values for feed rate
and depth of cut were used and based on the present investi-
gation, we can precisely select the optimum cutting conditions.
Table 4. Cutting force components [feed force (Fx), thrust force (Fy), and cutting force (Fz)], N.
Machining parameters Feed force (Fx), N Thrust force (Fy), N Cutting force (Fz), N
Ex. No. Vc, m/min f, mm/rev d, mm AR AC FC AR AC FC AR AC FC
1 35 0.02 0.5 83.74 104.29 72.09 92.71 116.22 81.06 166.69 168.78 161.62
2 35 0.04 0.5 87.77 106.42 83.89 98.74 121.48 92.84 215.30 225.06 169.62
3 35 0.06 0.5 93.14 114.85 87.07 102.11 138.81 100.09 224.85 312.01 201.29
4 45 0.02 0.5 64.25 98.4 60.25 73.24 106.87 71.63 155.64 160.20 124.08
5 45 0.04 0.5 79.52 95.84 67.37 91.48 109.8 78.38 172.00 220.07 151.92
6 45 0.06 0.5 84.49 100.23 77.01 99.57 115.08 93.01 212.12 255.07 183.78
7 55 0.02 0.5 62.42 70.47 59.24 69.2 83.77 65.23 106.99 148.99 101.38
8 55 0.04 0.5 64.32 76.84 61.65 76.2 91.67 71.69 160.95 206.80 120.30
9 55 0.06 0.5 70.74 81.36 65.24 80.71 95.89 76.94 188.90 226.81 134.80
Vc-cutting speed; f-feed rate; d-depth of cut; AR-As-received; AC-Air-cooled; FC-Furnace cooled
Moreover, the cutting speed range of 10–30 m/min is best amount of titanium carbides as precipitate particles are usually
suitable to turn nickel-based superalloys.[25] The exceeding formed during heat treatment of Incoloy 800H.[9,20] The
of cutting speed above 40 m/min would represent high-speed formed quantity of precipitate particles would mainly depend
machining for nickel-based alloys[25] and hence the cutting on temperature and time. However, the variation of precipitate
speed range of 35–55 m/min was used in this research. Nine particles (both amount and size) with the aging time is not the
turning experiments were conducted in each of AR, AC, and main objective of the present work. The combination of coarse
FC samples. Moreover, replications are needed to establish grains (∼75%) and fine grains (∼25%) was observed in the fur-
repeatability and authenticity of the data obtained during the nace-cooled samples [Figure 3(c)]. The observed average grain
experiment, so that the number of replications used in this size of the furnace-cooled sample was around 342 µm. The
experiments is 3 and average values have been reported. grain coarsening of furnace sample was attributed to slow
Further, the cutting force components (Table 4, Fx, Fy, and cooling rate started from high temperature (975°C) which
Fz) and the surface roughness (Ra) were measured as led to attain the room temperature slowly eventually grain
responses. These responses would mainly influence the quality growth would occur. The formed fine grains in the furnace-
of finished products after metal cutting and hence the atten- cooled sample were attributed to pinning of grain growth by
tion was focused on the present research work. Piezoelectric the precipitate particles.[18] Some twinning lines were observed
dynamometer coupled with a charge amplifier and data acqui- in both the heat-treated samples [Fig. 3(b) and (c)]. To
sition system (KISTLER type 9257B) was used to measure the confirm the presence of formed precipitate particles after heat
cutting force components [Fig. 1(b)]. KISTLER dynoware treatment, SEM micrograph of heat-treated furnace-cooled
software was used to interpret the results. The surface rough- sample is shown in Fig. 2(d) which was taken at high
ness (Ra) was also measured in the turned workpiece using magnification. The corresponding EDAX spectrum is shown
Mitutoyo surf test SJ-310 and 3D surface profiles were taken in Fig. 3(e) which demonstrates the presence of more amount
using the high-resolution white light interferometer. Table 3 of carbon, titanium, and chromium elements when compared
illustrates the measured experimental results. to the as-received chemical composition as mentioned in
Table 1. It is to be noted here that the amount of titanium
was lower than chromium which means more amount of
Results and Discussion
chromium carbides was expected to be formed when
The optical microstructures of Incoloy 800H superalloys of compared to titanium carbides.[11] The observed average size
as-received (AR) and heat-treated under different conditions of the precipitate was around 450 nm which was expected to
are shown in Fig. 3(a–c). The microstructure of as-received enhance the machinability and work hardening.
forged sample [Fig. 3(a)] was exhibited austenite equiaxed The variation of engineering compressive stress and
grains, ferrite grain boundaries with ferrite stringers. The pres- compressive strain curves for as-received (AR), air-cooled
ence of ferrite stringers would enhance the strength of the (AC), and furnace-cooled (FC) samples are shown in Fig. 4.
alloy due to which it would be very difficult to machine and The calculated compressive yield strength at 0.2% strain was
to use the alloy as-forged condition which needs heat treat- 472, 493, and 440 MPa for AR, AC, and FC samples, respect-
ment. Based on several optical images, the observed average ively. It was observed here that compressive yield strength of
grain size of the as-received forged sample was 182 µm. AC sample was exhibited more value which was 4.5% more
Figure 3(b) and (c) shows the microstructures of air-cooled than the as-received sample and 12% more than furnace-
and furnace-cooled samples, respectively. The air-cooled sam- cooled sample. The higher value of compressive yield strength
ple was exhibited somewhat fine grains [Fig. 3(b)] when com- for AC sample was attributed to the presence of fine grains,
pared to other two conditions [Fig. 3(a) and (c)]. The precipitates, and strain fields in the grains. Further, the
measured average grain size for the air-cooled sample was compressive yield strength for FC sample was around 7.2%
around 110 µm. The formation of fine grains in the air-cooled lower when compared to AR sample. This result was expected
sample was attributed to considerable fast cooling rate to the presence of coarse grains eventually it would soft the
occurred in the air medium and formed precipitates after matrix. The grain coarsening would occur in the furnace
heat treatment might have pinned down the grain growth. cooled sample because of the slow cooling rate occur in the
In general, more amount of chromium carbides and a small furnace which meant the sample would take more time to
MATERIALS AND MANUFACTURING PROCESSES 1597
Figure 3. Microstructures of Incoloy 800 H superalloy under different heat-treated conditions: (a) optical microstructures (OM) of as-received (AR); (b) OM of air
cooled (AC); (c) OM of furnace cooled (FC); (d) SEM of FC; (e) EDAX of (d).
reach the room temperature. However, the air-cooled sample more in yield strength. Moreover, the heat-treated samples had
would take considerable fast cooling which avoids grain shown more work hardening rate when compared to AR sam-
coarsening during heat treatment and hence it usually exhibits ple for the same 30% set height reduction. The microstructures
Figure 4. Engineering compressive stress and compressive strain curve of Incoloy 800H superalloy of as-received, air-cooled, and furnace-cooled conditions
(corresponding deformed microstructures, samples of un-deformed and deformed).
1598 A. PALANISAMY ET AL.
of deformed samples clearly demonstrated (Fig. 4) that more The cutting force components (Fx, Fy, and Fz) attained
elongated with almost equiaxed grains were observed in both during machining of as-received forged condition and differ-
heat-treated samples when compared to AR sample. The ent heat-treated conditions are listed in Table 1. The variation
formed nanoprecipitates (∼450 nm) were expected to enhance of cutting force (Fz) on the cutting speed and feed rate with
more strain hardening rate in the heat-treated samples. different heat-treated conditions is shown in Fig. 6. It was
Further, the AC sample of the compressive stress–strain curve found that air-cooled sample exhibited more cutting force
was shifted up (Fig. 4) due to the presence of fine grains in the values when compared to other two different conditions in
matrix and more amount of strain fields. The compressive all the tested cutting parameters. This result was expected to
stress–strain curve for FC sample was shifted down when the presence of fine grains in the matrix and higher value of
compared to other two conditions. This was expected to the mechanical strength. In contrast, the furnace-cooled sample
existing of coarse grains in the matrix and lower amount of exhibited less cutting force values when compared to other
strain fields.[26] two different conditions in all the tested cutting parameters.
To examine the fracture analysis on the deformed samples This result was attributed to the presence of coarse grains,
at room temperature, the deformed samples were pierced more amounts of precipitates, and lower value of mechanical
lengthways which were parallel to the applied load strength. However, the as-received forged conditioned sample
direction.[27] Figure 5 shows the SEM fractography of all the had shown more value of cutting force when compared to
three samples which are processed under different conditions. furnace-cooled sample. This was attributed to ferrite stringers
The fracture surface of as-received forged condition [Fig. 5(a)] and somewhat lesser grain size in the matrix compared to
shows dimples, craters, and crocodile patterns. The presence furnace-cooled sample. The range of cutting force components
of dimples would associate with the ductility, whereas the values (Fz) was 106.99–224.85 N for AR condition, 148.99–
presence of more craters and crocodile patterns would associ- 312.01 N for AC condition, and 101.38–201.29 N for FC
ate with the brittleness nature. The observed crocodile patterns condition. Figure 6(a) shows the variation of cutting force with
and more craters in the as-received forged sample were the function of feed rate at V ¼ 35 m/min for instance,
attributed to the ferrite stringers in the matrix. Deep dimples, whereas Fig. 6(b) shows the variation of cutting force with
the large crater, flat surface-fractured zone, and voids were the function of cutting speed at f ¼ 0.02 mm/rev. These two
observed in the air-cooled sample [Fig. 5(b)]. The formation graphs [Fig. 6(a) and (b)] were drawn on the same y-axis scale
of a flat surface-fractured zone was attributed to fine grains in which the average cutting force of 200N was mentioned.
and more amount of strain fields in the matrix. The formation Figure 6(a) demonstrates clearly that air-cooled sample
of voids was attributed to the pullout of precipitates. However, influenced more followed by the as-received sample. However,
deformed cum coalesced dimples, river pattern fractured the furnace-cooled sample had exhibited lower cutting forces
zone, and voids were observed in the furnace-cooled sample and it was not influenced much by the function of feed rate.
[Fig. 5(c)]. The deformed cum coalesced dimples and the This was expected to the presence of coarse grains and preci-
river pattern-fractured zone was associated with more in pitates in the matrix. Further, the cutting force had started to
deformation and work hardening occurred in the sample. increase with the function of feed rate under all the conditions.
The deformed cum coalesced dimples were attributed to The increasing trend of cutting force with the feed rate was
coarse grains and fewer strain fields in the matrix.[26] attributed to more friction occurred amidst the tool and the
Figure 5. SEM fracture surface of Incoloy 800 H under different conditions: (a) as-received (AR); (b) air-cooled (AC); and (c) furnace-cooled (FC).
MATERIALS AND MANUFACTURING PROCESSES 1599
Figure 6. Variation of cutting force (Fz) of Incoloy 800 H under different conditions: (a) at cutting speed, V ¼ 35 m/min; (b) at feed rate, f ¼ 0.02 mm/rev.
workpiece in addition to the effect of grain size, ferrite This was attributed to more mechanical strength and some-
stringers, and amount of precipitates. Similar behavior what smaller grain size when compared to furnace-cooled
was seen for the other values of cutting speed (45 and sample. However, the furnace-cooled sample had shown neg-
55 m/min). Figure 6(b) explains legibly that the cutting speed ligible grooves only which indicated that a good surface finish
was not influenced much by the cutting force when compared was obtained in the furnace-cooled sample. This result was
to the feed rate. However, the cutting force had started to expected to the presence of coarse grains, precipitates, and
decrease with the cutting speed under all the conditions. The lower value of mechanical strength. These results were
reduction of cutting force was attributed to thermal softening explained that the coarse grains, amount of precipitates, and
that occurs because of high temperature at the machining low value of mechanical strength in the Incoloy 800H had
zone. However, the furnace-cooled sample had exhibited the promoted immediate shearing action which resulted in a good
very low value of cutting force when compared to other two surface finish. The range of surface roughness obtained from
conditions. This was expected to the presence of coarse grains, the experiments under different heat-treated conditions is
lower mechanical strength value, and precipitates in the matrix 0.82–1.66 µm for AR, 1.30–2.08 µm for AC, and 0.30–1.03 µm
in addition to thermal softening. Similar behavior was noticed for FC. Figure 8 shows the variation of surface roughness with
for the other values of feed rate (0.04 and 0.06 mm/rev). The the function of the feed rate at V ¼ 35 m/min and the cutting
results exhibited by feed force (Fx) and thrust force (Fy) with speed at f ¼ 0.02 mm/rev as an example. Figure 8(a) clearly
the variation of cutting parameters were similar in trend pro- demonstrates that the surface roughness value started to
duced by cutting force (Fz). As discussed, the heat treatment increase with the function of feed rate. This was attributed
process given to the Incoloy 800H had formed the precipitates, to increasing of successive tool path gaps which led to produc-
produced different grain sizes, and varied the material’s mech- ing more peak and valley height in the turned profile. The
anical strength; eventually, it had improved its machinability higher value of peak and valley height indicated more in
when compared to the as-received forged condition. These surface roughness value which meant poor in surface finish.
results were well correlated with the other researchers found Both air-cooled and as-received conditioned samples were
in elsewhere.[28,29] influenced more by the function of feed rate when compared
Surface quality plays a significant role in fatigue life and
performance of the machined parts. Table 1 illustrates the
surface roughness of the machined samples under various
heat-treated conditions. Figure 6 shows the 3D surface profile
obtained from the high-resolution white light interferometer
for the machined sample of AR [Fig. 7(a)], AC [Fig. 7(b)],
and FC [Fig. 7(c)] at the higher cutting speed (55 m/min)
and the lower feed rate (0.02 mm/rev) as an example. In
general, the plowing effect of cutting tool insert would greatly
influence the surface finish of the machined components. This
plowing effect would cause small grooves on the machined
surfaces and hence it has to be minimized. It was found
from 3D surface profiles (Fig. 7) that the air-cooled samples
[Fig. 7(b)] had exhibited more small groves when compared
to other two samples [Fig. 7(a) and (c)]. These results were
explained that severe plowing effect had occurred in the air-
cooled sample due to more strain fields and higher value of
Figure 7. 3D surface profile of the machined samples with different
mechanical strength. Further, the as-received forged con- conditions at V ¼ 55 m/min and f ¼ 0.02 mm/rev: (a) as-received; (b) air cooled;
ditioned sample also had shown some severe grooves. and (c) furnace cooled.
1600 A. PALANISAMY ET AL.
Figure 8. Variation of surface roughness (Ra) of Incoloy 800 H under different conditions: (a) at cutting speed, V ¼ 35 m/min; (b) at feed rate, f ¼ 0.02 mm/rev.
to furnace-cooled sample. Similar behavior was noticed for the . Incoloy 800H under air-cooled condition had induced
other cutting speeds (45 and 55 m/min). However, decreasing higher cutting force (312.01 N) when compared with under
of surface roughness with the function of cutting speed under furnace-cooled condition (201.21 N) during the dry turning
different heat-treated conditions is shown in Fig. 8(b). Here operation.
also, the furnace-cooled sample had exhibited a very low value . The observed surface roughness was better at
of surface roughness when compared to the other two different V ¼ 55 m/min and f ¼ 0.02 mm/rev than other combina-
conditions. Similar behavior was noticed for the other feed tions of selected parameters. The better surface finish was
rates (0.04 and 0.06 mm/rev). In general, the temperature obtained during the machining of the sample under
would start to increase as the cutting speed increases which furnace-cooled condition.
leads to producing thermal softening between the tool and . Incoloy 800H superalloy under furnace-cooled (FC) con-
work material.[9,30] Due to this thermal softening effect at dition had provided better machinability compared with
higher cutting speed, the observed surface roughness value AC and AR samples at V ¼ 55 m/min and f ¼ 0.02 mm/rev.
was low in all the samples. Based on Fig. 8, it can be
concluded that a good surface finish was obtained in the fur- ORCID
nace-cooled sample due to the presence of coarse grains and
precipitates, and its lower mechanical strength value, whereas S. Sivasankaran http://orcid.org/0000-0002-7456-375X
poor in the surface finish was obtained in the air-cooled
sample due to the high mechanical strength value. References
[1] Hayner, G. O.; Shaber, E. L.; Mizia, R. E.; Bratton, R. L.; Sowder, W. K.;
Conclusion Wright, R. N.; Windes, W. E.; Totemeier, T. C.; Moore, K. A. Next Gen-
eration Nuclear Plant Materials Research and Development Program
In this analysis, the interaction between microstructure, Plan; Idaho National Engineering and Environmental Laboratory,
material property, and machinability on dry turning as a result Bechtel BWXT Idaho, LLC, 2004 (INEEL/EXT-04–02347), USA.
of the effect of heat treatment in an Incoloy 800H with [2] Pervaiz, S.; Rashid, A.; Deiab, I.; Nicolescu, M. Influence of
uncoated carbide tool inserts were elaborately investigated Tool Materials on Machinability of Titanium- and Nickel-Based
Alloys: A Review. Mater. Manuf. Process. 2014, 29(3), 219–252.
and reported. The following concluding points were drawn, DOI: 10.1080/10426914.2014.880460.
relating to the selected parameters and the experimental [3] Wang, X.; Huang, C.; Liu, H.; Zhu, H.; Wang, J. A New Method to
results. Evaluate the Machinability of Difficult-To-Cut Materials. Int. J. Adv.
. The microstructural analysis in terms of grain size, grain Manuf. Technol. 2014, 75(1–4), 91–96.
size distribution, and twins were explained clearly. These [4] Chavosh, S. Z.; Tajdari, M. Surface Roughness Modeling in Hard
Turning Operation of AISI 4140 Using CBN Cutting Tool. Int. J.
results explained that fine grains were observed in the air- Mater. Forming 2010, 3, 233–239.
cooled sample, whereas coarse grains were observed in [5] Handbook, A. S. M. Volume 16: Machining, ASM International
the furnace-cooled sample Handbook Committee; ASM International, Electronic: Ohio, OH,
. The formation of chromium carbides as precipitates was 1989; p 690.
confirmed through SEM analysis on the furnace-cooled [6] Khan, S. A.; Ahamad, M. A.; Saleem, M. Q.; Asif, M.; Qureshi, M.
High-Feed Turning of AISI D2 Tool Steel Using Multi-Radii
sample. The size of the grain, the amount of precipitates, Tool Inserts: Tool Life, Material Removed, and Workpiece Surface
and strain fields had defined the strength of the sample in Integrity Evaluation. Mater. Manuf. Process. 2017, 32(6), 670–677.
which air-cooled sample had shown more mechanical DOI: 10.1080/10426914.2016.1232815.
strength due to its finer grain size and more amount of [7] Palanisamy, D.; Senthil, P. Development of ANFIS Model and
strain fields. Machinability Study on dry Turning of Cryo-Treated PH Stainless
Steel with Various Inserts. Mater. Manuf. Process. 2017, 32(6),
. The observed lower value of mechanical strength in the 654–669. DOI: 10.1080/10426914.2016.1221091.
furnace-cooled sample was attributed to the presence of [8] Radhika, N.; Subramaniam, R.; Senapathi, S.B. Machining Parameter
coarse grains and precipitates in the matrix. Optimization of an Aluminium Hybrid Metal Matrix Composite by
MATERIALS AND MANUFACTURING PROCESSES 1601
Statistical Modelling. Ind. Lubrication Tribol. 2013, 65(6), 425–435. [20] Gaitonde, V. N.; Karnik, S. R.; Figueira, L.; Paulo Davim, J. Analysis
DOI: 10.1108/ilt-01-2011-0008. of Machinability During Hard Turning of Cold Work Tool Steel
[9] Aouici, H.; Yallese, M. A.; Chaoui, K.; Mabrouki, T.; Rigal, J. F. (Type: AISI D2). Mater. Manuf. Process. 2009, 24, 1373–1382.
Analysis of Surface Roughness and Cutting Force Components in DOI: 10.1080/10426910902997415.
Hard Turning with CBN Tool: Prediction Model and Cutting [21] Palanisamy, A.; Selvaraj, T.; Sivasankaran, S. Taguchi-Based Grey
Conditions Optimization. Measurement 2012, 45(3), 344–353. Relational Analysis for Modeling and Optimizing Machining
DOI: 10.1016/j.measurement.2011.11.011. Parameters Through Dry Turning of Incoloy 800H. J. Mech. Sci.
[10] Klocke, F.; Nobel, C.; Veselovac, D. Influence of Tool Coating, Tool Technol. 2017, 31(9), 4159–4165.
Material, and Cutting Speed on the Machinability of Low-Leaded [22] Imran Ansari, M. D.; Kotiveerachary, B. Study of the Effect of
Brass Alloys in Turning, Mater. Manuf. Process. 2016, 31(14), Minimum Quantity Lubrication on the Surface Roughness of
1895–1903. DOI: 10.1080/10426914.2015.1127944. Incoloy 800 During Turning Operation. Int. J. Curr. Eng. Technol.
[11] Senthil, P.; Selvaraj, T.; Sivaprasad, K. Influence of Turning 2014, 2, 18–22.
Parameters on the Machinability of Homogenized Al–Cu/TiB2 [23] Poulachon, G.; Moisan, A. L. Hard Turning: Chip Formation
In-Situ Metal Matrix Composites. Int. J. Adv. Manuf. Technol. Mechanisms and Metallurgical Aspects. AJSME 2000, 122, 406–412.
2013, 67(5–8), 1589–1596. [24] Aneiro, F. M.; Coelho, R. T.; Brandao, L. C. Turning Hardened Steel
[12] Sharma, V.; Pandey, P. M. Comparative Study of Turning of Using Coated Carbide at High Cutting Speeds. J. Braz. Soc. Mech.
4340 Hardened Steel with Hybrid Textured Self-Lubricating Sci. Eng. 2008, 30(2), 104–109.
Cutting Inserts. Mater. Manuf. Process. 2016, 31(14), 1904–1916. [25] Dudzinski, D.; Devillez, A.; Moufki, A.; Larrouquère, D.; Zerrouki,
DOI: 10.1080/10426914.2015.1127951. V.; Vigneau, J. A Review of Developments Towards Dry and High
[13] Ferreira, R.; Carou, D.; Lauro, C. H.; Davim, J.P. Surface Roughness Speed Machining of Inconel 718 Alloy. Int. J. Mach. Tools Manuf.
Investigation in the Hard Turning of Steel Using Ceramic Tools. 2004, 44, 439–456.
Mater. Manuf. Process. 2016, 31(5), 648–652. DOI: 10.1080/ [26] Shi, B.; Attia, H.; Tounsi, N. Identification of Material Constitutive
10426914.2014.995051. Laws for Machining-Part I: An Analytical Model Describing the
[14] Khanna, N.; Sangwan, K. S. Comparative Machinability Study on Stress, Strain, Strain Rate, and Temperature Fields in the Primary
Ti54 M Titanium Alloy in Different Heat Treatment Conditions. Shear Zone in Orthogonal Metal Cutting. J. Manuf. Sci. Eng.
Proc. Inst. Mech. Eng., Part B 2013, 227(1), 96–101. 2010, 132(5), 051008–051011.
[15] Lokesh, K. S.; Pinto, T.; Ramachandra, C. G. Effect of Tool Wear & [27] Senkov, O. N.; Wilks, G. B.; Scott, J. M.; Miracle, D. B. Mechanical
Machinability Studies on Polymer Composites: A Review. Int. J. Eng. Properties of Nb25Mo25Ta25W25 and V20Nb20Mo20Ta20W20
Inf. Syst. 2017, 1(5), 71–77. Refractory High Entropy Alloys. Intermetallics 2011, 19, 698–706.
[16] Polishetty, A.; Littlefair, G.; Goldberg, M.; Nomani, J. Current DOI: 10.1016/j.intermet.2011.01.004.
Trends in Machinability Research. Int. J. Mater. Form. Mach. [28] Das, S. R.; Dhupal, D.; Kumar, A. Experimental Investigation into
Process. 2016, 3(1), 1–11. Machinability of Hardened AISI 4140 Steel Using TiN Coated
[17] Ueno, T.; Yamada, K. Study on the Difference of Machinability Between Ceramic Tool. Measurement 2015, 62, 108–126.
Iron-Based Sintered Materials and Steel Materials. Mater. Sci. Forum [29] Amini, K.; Hoda, M. R.; Shafyei, A. Investigation of the Effect
2016, 874, 433–438. DOI: 10.4028/www.scientific.net/msf.874.433. of Heat Treatment on the Mechanical Properties and
[18] Veiga, C.; Davim, J. P.; Loureiro, A. J. R. Review on Machinability of Microstructure of DIN 1.4057 Martensitic Stainless Steel. Metal
Titanium Alloys: The Process Perspective. Rev. Adv. Mater. Sci. Sci. Heat Treat. 2014, 55(9–10), 499–503. DOI: 10.1007/
2013, 34(2), 148–164. s11041-014-9661-9.
[19] Suresh, R.; Basavarajappa, S.; Samuel, G.L. Some Studies on Hard [30] Suresh, R.; Basavarajappa, S.; Gaitonde, V. N.; Samuel, G. L.
Turning of AISI 4340 Steel Using Multilayer Coated Carbide Tool. Machinability Investigations on Hardened AISI 4340 Steel Using
Measurement 2012, 45(7), 1872–1884. DOI: 10.1016/j.measurement. Coated Carbide Insert. Int. J. Refract. Met. Hard Mater. 2012, 33,
2012.03.024. 75–86. DOI: 10.1016/j.ijrmhm.2012.02.019.