Professional Documents
Culture Documents
Solid FLAC Cement Fluid-Loss Additive: Robust Formulation
Solid FLAC Cement Fluid-Loss Additive: Robust Formulation
■■
80
60
■■ 60
40
API fluid
40
20
20
0
0.2 0.3 0.4 0.5 0.6
0
0.2 0.3D255 concentration,
0.4 % BWOC 0.5 0.6
60 0.6
50
0.55
mL/30mL/30
50 0.4
40
fluid loss,
40 0.4
30
API loss,
30
20
API fluid
20
10
10
0
0 5 10 18
0 NaCl concentration, % BWOW
0 5 10 18
NaCl concentration, % BWOW
The D255 concentration (shown in % BWOC) required to reach an approximate API fluid
loss of 50 mL/30 min varies with the mix-water salinity, expressed here as a percentage
by weight of water (% BWOW).