net/publication/322889908
Determination of the most efficient form of sulfur for use as a natural rubber
curing agent by comparison of physical and thermal attributes of cured rubber
CITATIONS READS
2 208
2 authors:
Some of the authors of this publication are also working on these related projects:
All content following this page was uploaded by Hedieh Shahrampour on 01 December 2019.
89
90 ALIREZA MOTAVALIZADEHKAKHKY, HEDIEH SHAHRAMPOUR
71.0 140
70.8 134.6
135
70.6 70.5
70.4 130
70.2 125
70.0
14 12.81
12 IS-NR
11.47
10 RS-NR
8.81
8.03
8
%
300
258.6 IS-NR
250 RS-NR
205.15
200
150
100
50
0
90 84.6
80 IS-NR
70 RS-NR
60 54.1
50
40 38.8
30 27.5
20
10
1.8 0.65
0
the changes of elongation the changes the changes of hardness
of tensile strength
%
14 12.8
35 32.2 12 IS-NR
30 IS-NR 9.7 RS-NR
25.2 10
25 RS-NR
N/mm
20 8
15 6
10 4
5 2
0 0
Fig. 6. Force required to tear specimens. Fig. 7. The results of the compression set.