Download as xls, pdf, or txt
Download as xls, pdf, or txt
You are on page 1of 12

Dhaka khulna (N8) Road Improvement Project

HQ,24 Engineer Construction Brigade ,Bangladesh Army.


Package-3

Consultant: Contractor:
HPCPDIL PDL-CAMCE-CR-24B= JV

Flakiness Index (BS-812)


Lab Ref. No. : Sample No. : 03

Source : India Date of sampling : 08.08.18

Description : 16 mm Pakur Stone Chips Date of testing : 12.08.18

Sample Location :Stackyard Purpose : Binder Course Mix Design

Wt. of sample : 4545 gm Sampled by : Jointly

Sieve Size
Test Weight (gm) Weight Passing (gm) % Flaky Remarks
(mm)

63.0-50.0
50.0-37.5
37.5-28.0
28.0-20.0
20.0-14.0 2527 620 24.54
14.0-10.0 1874 270 14.41
10.0-6.30 144 63 43.75
Total 4545 953 20.97

total weight passing thickness gauge x 100


Flakiness Index =
Total weight of test sample

= 20.97 % ≈ 21%

Technician Material Engineer Material Engineer Representative


Technician Consultant Consultant
Contractor Contractor HQ,24-ECB
Technician Material Engineer Material Engineer Representative
Technician Consultant Consultant
Contractor Contractor HQ,24-ECB
9.5mm 100 100

4.75mm 95 100
2.36mm 80 100
1.18mm 50 85
0.600mm 25 60
0.300mm 10 30
0.150mm 2 10
Dhaka khulna (N8) Road Improvement Project
HQ,24 Engineer Construction Brigade ,Bangladesh Army.
Package-3

Consultant: Contractor:
HPCPDIL PDL-CAMCE-CR-24B= JV

Flakiness Index (BS-812)


Lab Ref. No. : Sample No. : 02

Source : India Date of sampling : 08.08.18

Description : 20mm Pakur Stone Chips Date of testing : 11.08.18

Sample Location :Stackyard Purpose : Binder Course Mix Design

Wt. of sample : 4528 gm Sampled by : Jointly

Sieve Size
Test Weight (gm) Weight Passing (gm) % Flaky Remarks
(mm)

63.0-50.0
50.0-37.5
37.5-28.0
28.0-20.0
20.0-14.0 2510 410 16.33
14.0-10.0 1874 290 15.47
10.0-6.30 144 63 43.75
Total 4528 763 16.85

total weight passing thickness gauge x 100


Flakiness Index =
Total weight of test sample

= 16.85 % ≈ 17%

Technician Material Engineer Material Engineer Representative


Technician Consultant Consultant
Contractor Contractor HQ,24-ECB
Technician Material Engineer Material Engineer Representative
Technician Consultant Consultant
Contractor Contractor HQ,24-ECB
9.5mm 100 100

4.75mm 95 100
2.36mm 80 100
1.18mm 50 85
0.600mm 25 60
0.300mm 10 30
0.150mm 2 10
Dhaka khulna (N8) Road Improvement Project
HQ,24 Engineer Construction Brigade ,Bangladesh Army.
Package-3

Consultant: Contractor:
HPCPDIL PDL-CAMCE-CR-24B= JV

Flakiness Index (BS-812)


Lab Ref. No. : Sample No. : 04

Source : India Date of sampling : 08.08.18

Description : 10 mm Pakur Stone Chips Date of testing : 12.08.18

Sample Location :Stackyard Purpose : Binder Course Mix Design

Wt. of sample : 1383 gm Sampled by : Jointly

Sieve Size
Test Weight (gm) Weight Passing (gm) % Flaky Remarks
(mm)

63.0-50.0
50.0-37.5
37.5-28.0
28.0-20.0
20.0-14.0
14.0-10.0 783 80 10.22
10.0-6.30 600 140 23.33
Total 1383 220 15.91

total weight passing thickness gauge x 100


Flakiness Index =
Total weight of test sample

= 15.91 % ≈ 16%

Technician Material Engineer Material Engineer Representative


Technician Consultant Consultant
Contractor Contractor HQ,24-ECB
Technician Material Engineer Material Engineer Representative
Technician Consultant Consultant
Contractor Contractor HQ,24-ECB
9.5mm 100 100

4.75mm 95 100
2.36mm 80 100
1.18mm 50 85
0.600mm 25 60
0.300mm 10 30
0.150mm 2 10
Dhaka khulna (N8) Road Improvement Project
HQ,24 Engineer Construction Brigade ,Bangladesh Army.
Package-3

Consultant: Contractor:
HPCPDIL PDL-CAMCE-CR-24B= JV

Flakiness Index (BS-812)


Lab Ref. No. : Sample No. : 01

Source : India Date of sampling : 08.08.18

Description : 25mm Pakur Stone Chips Date of testing : 11.08.18

Sample Location :Stackyard Purpose : Binder Course Mix Design

Wt. of sample : 5257 gm Sampled by : Jointly

Sieve Size
Test Weight (gm) Weight Passing (gm) % Flaky Remarks
(mm)

63.0-50.0
50.0-37.5
37.5-28.0
28.0-20.0 1012 297 29.35
20.0-14.0 2527 410 16.22
14.0-10.0 1574 230 14.61
10.0-6.30 144 63 43.75
Total 5257 1000 19.02

total weight passing thickness gauge x 100


Flakiness Index =
Total weight of test sample

= 19.02 % ≈ 19%

Technician Material Engineer Material Engineer Representative


Technician Consultant Consultant
Contractor Contractor HQ,24-ECB
Technician Material Engineer Material Engineer Representative
Technician Consultant Consultant
Contractor Contractor HQ,24-ECB
9.5mm 100 100

4.75mm 95 100
2.36mm 80 100
1.18mm 50 85
0.600mm 25 60
0.300mm 10 30
0.150mm 2 10

You might also like