a
WY/MHOD/ISYH : GYOOSY
HVYMOH ‘HUVOVINHC ‘Helv TSLISNONI TIVINYS
) S3IWLSNGNI 1431L$"8"H >
“WISLVINMVa = 404d Luodau 1Sa)
7 —+—"
- — |
: > Toh
ff |
_ _| ||
WD VP OP 99 “BOOLS TI Fw | reoor \gqve7 ee a
(wtos | ("R %09 "per jnowyHS
SER pores | ee | RRS) (lows edn | xouvonsay | scvio “| onsen wee wea mr |
] PLT ~_ NOISNAHTG
RAP ormsnrs WAVY TIT ATONE “oxo ION
‘ . LOhVET <7~H TI OGOGIGT 301
se /asfreva/ cof [wpe lm fee pm pe pw [
3 win, fossofoeof | —-|—-]|—]-] =|] 1] = Joos
can rontents «pom! | Rrarogen caygen wicrogen
Mechanical Properties
a fe wcaness | omer tate | cosaraot _|'seap om cart [notte
coniition|"on'te | cxg/mmey [22°] % | 4 | actieay weges an per os pes 2554075] re
(pun) | Tz0d/ Charpy = cure meme | argent
eens [aR : =p om aE
|Netaiiurgical Test
iam reset) | BEI 7 | oecero tom | Ae pe . : < 2
beetdined BE: T # T H T a
hero Structure: Ferrite + peariite
““[Hardenability test (JOMINY TEST) 1 406
pias. wen
requaree =
[Actual pee
lNon Destructive Test
ecepared By: For Bhushan Power € steel ztd
ecanrsan Certified that the test findings are cserect’ and Oe
nased on actual result carried on samples drawn as per qu:
tan. Tathorived Bigeatoay
(oanlity asmurence)H.R.STEEL INDUSTRIES
Date 7 Time: 11:05:14 AM
Sample 32 MM COIL, CUSTOMER BPSL Call ID 22E2048,
c s P M
a Si cr Mo Al B
% % % % % %
Value 0.202 0.00312 0.00672 0.818 0.0692 0.184 0.00011 0.0286 0.00206