Oteluri
Oteluri
www.asminternational.org
Notes
Cr
Mn
0.15
max
17-20
2 max
0.15
max
17.019.0
2.00
max
Mo
Ni
Si
Other
8-11
0.04
max
0.03
max
0.5-2
Pb <=0.15; Ti>=5C;
bal Fe
8.010.0
0.04
max
0.03
max
1.00
max
bal Fe
UTS YS El
Hard
T15NiCr180
Corr res
USA
UNS J92501
MIL-S-81591(93)
IC-302*
bal Fe
60303
IC-303*
AMS 5341C(95)*
MIL-S-81591(93)
0.12
max
0.16
max
0.16
max
17.020.0
18.0021.00
18.0021.00
2.00
max
2.00
max
2.00
max
0.60
max
0.80
max
0.75
max
8.010.0
9.0021.00
9.0012.00
0.17
max
0.04
max
0.04
max
0.150.35
0.150.35
0.150.35
1.00
max
2.00
max
2.00
max
Cu <=0.50; bal Fe
Cu <=0.50; bal Fe
Cu <=0.75; bal Fe
180 HB
max
bal Fe
364C11*
Press ves
0.07
max
20.024.0
0.03
max
0.03
max
0.08
max
18.020.0
2.00
max
0.04
max
0.03
max
1.00
max
USA
UNS J92610
MIL-S-81591(93)
IC-304*
8.012.0
bal Fe
bal Fe
000CH18N11
Corr res
0.03
max
17-19
2 max
0.02
max
GX2CrNi1910
0.03
max
17-21
1.5 max
8-12
0.04
max
0.035
max
2 max
304S12*
0.03
max
17-21
2 max
0.04
max
0.04
max
UNS J92620
0.05
max
18.021.0
1.002.00
8.011.0
0.04
max
0.03
max
1.00
max
Italy
UNI 3161(83)
bal Fe
UK
BS 1504(76)
USA
MIL-S-81591(93)
IC-304L*
0.50
max
Cu <=0.50; bal Fe
bal Fe
310C40*
Press ves
0.3-0.5 24.027.0
19.022.0
0.04
max
0.04
max
UNS J94302
310
0.25
max
2.00
max
19.022.0
0.04
max
0.03
max
1.00
max
IC-310*
USA
MIL-S-81591(93)
24.026.0
bal Fe
bal Fe
G-X2CrNiMoN18 14 Non-magnetic
0.03
max
16.518.5
2.00
max
2.503.00
13.015.0
0.045
max
0.015
max
1.00
max
N 0.15-0.25; bal Fe
490- 295
690
30
UNS numbers and US grades are provided as a means of cross referencing chemically similar alloys. Exchangability is only possible after independent examination of specifications. Tensile properties are minimum or typical as
specified. UTS and YS as MPa. El as %. See Appendix for list of abbreviations used in Notes. * indicates obsolete material.
www.asminternational.org
Notes
Cr
Mn
Mo
Ni
Si
0.045
max
0.015
max
1.00
max
Other
UTS YS El
Hard
WNr 1.3952
Non-magnetic
0.03
max
16.518.5
2.00
max
2.503.00
13.015.0
N 0.15-0.25; bal Fe
316C71*
Press ves
0.08
max
17.021.0
0.04
max
0.04
max
UNS J92810
316
0.08
max
16.018.0
2.00
max
2.0-3.0 10.014.0
0.04
max
0.03
max
1.00
max
bal Fe
0.035
max
0.035
max
0.03
max
0.03
max
1 max
Pb <=0.15; Nb>=8C;
bal Fe
Pb <=0.15; Ti
<=1.30; Ti>=5C; bal
Fe
490- 295
690
30
460
20L 140210HB
160-230
HB
20L 140-210
HB
160-230
HB
20L 140-210
HB
UK
BS 1504(76)
USA
2 max
2-2.5
10-13
STAS 9277(84)
2 max
2-2.5
10-13
UNS J92920
0.040.10
16.018.0
2.00
max
2.003.00
11.014.0
0.040
max
0.030
max
0.75
max
12-15
0.035
max
0.02
max
1 max
USA
316H
bal Fe
000CH17N14M2
Corr res
0.03
max
16-18
2 max
2-2.5
UNS J92804
CF3MN
CF3MN
Corr res
0.03
max
0.03
max
17.022.0
17.022.0
1.50
max
1.50
max
2.0-3.0 9.013.0
2.0-3.0 9.013.0
0.040
max
0.040
max
0.040
max
0.040
max
1.50
max
1.50
max
0.15
max
0.15
max
0.15
max
0.15
max
0.15
max
17-19
2 max
2-3
9-11
2 max
2-3
9-11
17-19
2 max
2-3
9-11
17-19
2 max
8-11
17-19
2 max
8-11
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
17-19
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
UNS J92630
0.08
max
17.019.0
2.00
max
9.012.0
0.04
max
0.03
max
1.00
max
USA
ACI
N 0.10-0.20; bal Fe
N 0.10-0.20; bal Fe
200
200
200
USA
MIL-S-81591(93)
IC-321*
IC-347*
0.08
max
17.019.5
2.00
max
9.013.0
0.04
max
0.03
max
1.00
max
0.040.10
17.020.0
2.00
max
9.0013.0
0.040
max
0.030
max
0.75
max
UNS numbers and US grades are provided as a means of cross referencing chemically similar alloys. Exchangability is only possible after independent examination of specifications. Tensile properties are minimum or typical as
specified. UTS and YS as MPa. El as %. See Appendix for list of abbreviations used in Notes. * indicates obsolete material.
www.asminternational.org
Notes
Cr
Mn
Mo
Ni
0.040.10
0.040.10
18.021.0
18.021.0
1.50
max
1.50
max
0.15
max
0.15
max
17-19
2 max
8-12
17-19
2 max
8-11
0.8-2.0
8.011.0
Si
Other
0.040
max
0.040
max
0.040
max
0.040
max
1.50
max
1.50
max
bal Fe
0.04
0.04
2 max
bal Fe
UTS YS El
Hard
ACI
UNS J92901
Cr-Ni-Mo CF-10M
CF-10M
Cr-Ni-Mo
2.0-3.0 9.012.0
2.0-3.0 9.012.0
bal Fe
Ch18N10SL
Corr res
BDS 9631
Ch19N9L
Corr res
ZG1Cr18Ni9
0.12
max
17.020.0
Corr res
0.12
max
8-10
0.12
max
0.12
max
0.15
max
0.15
max
0.1-0.2
17.019.5
17.019.5
16.518.5
16.518.5
18-20
1.50
max
1.50
max
2.00
max
2.00
max
1.5 max
8.0010.0
8.0010.0
10.012.0
10.012.0
9-11
0.16
max
17-19
1 max
8-10
China
GB 2100(80)
0.045
max
0.030
max
441
196
25
440- 175
640
440- 175
640
20
480
26
France
AFNOR NFA35586 Z10CN18.9M
2 max
bal Fe
2.00
max
2.00
max
1.00
max
1.00
max
1.5-2.5
bal Fe
Germany
DIN
GX10CrNi18-8
DIN
WNr 1.4312
G-X12CrNi18 11
Non-magnetic
WNr 1.3955
Non-magnetic
TGL 10414
TGL 14415
GSF-X12CrNi189*
0.75
max
0.75
max
0.045
max
0.045
max
0.045
max
0.045
max
0.030
max
0.030
max
0.030
max
0.030
max
bal Fe
20
bal Fe
bal Fe
bal Fe
Mexico
DGN B-354
CF-16F*
0.16
18-21
1.5
9-12
0.04
0.04
bal Fe
LH18N9
Corr res
0.15
max
17-19
2 max
8-11
0.035
max
0.035
max
2 max
bal Fe
STAS 6855
T15NiCr180X
Corr res
17-19
2 max
8-10
0.5-2
bal Fe
STAS 6855(86)
T15NiCr180
17-20
2 max
8-10
STAS 6855(86)
T15TiNiCr180
0.15
max
0.15
max
0.15
max
17-19
2 max
8-12
GOST
10Ch18N9L
Corr res
17-20
1-2
8-11
GOST
10Ch18N9MLS
Corr res
17-20
1-1.8
0.1-0.2 8-11
BS 3100(91)
302C25
BS 3146/2(75)
ANC3(A)
17.021.0
17.020.0
2.00
max
0.202.00
8.00
min
8.0012.0
0.16
max
Corr res
0.16
max
Noncurrent; Corr res 0.16
max
Corr res; Solution Q/A 0.16
max
Corr res; Solution Q/A 0.16
max
18.021.0
18.021.0
18.0021.00
18.021.0
18.021.0
1.50
max
1.50
max
2.00
max
1.5 max
Poland
PNH83158(86)
Romania
0.04
max
0.035
max
0.03
max
0.03
max
0.5-2
Pb <=0.15; bal Fe
2 max
Pb <=0.15; Ti <=0.8;
5(C-0.03)<=Ti<=0.8;
bal Fe
0.035
0.03
0.2-1
bal Fe
0.02
0.02
0.2-1
Cu 0.3; bal Fe
0.040
max
0.035
max
0.040
max
0.035
max
1.50
max
0.202.00
bal Fe
0.04
max
0.04
max
0.04
max
0.17
max
0.04
max
0.04
max
0.04
max
0.150.35
0.04
max
0.200.40
2.00
max
2.00
max
2.00
max
2.00
max
2.00
max
bal Fe
Russia
0.070.14
0.140.7
UK
bal Fe
USA
UNS J92701
ACI
CF-16F
AMS 5341C(95)*
ASTM
A743/A743M(98)
ASTM
A743/A743M(98)
CF-16F
CF-16Fa
9.012.0
3.0 max 9.012.0
0.75
9.00max
12.00
1.50
9.0max
12.0
1.5 max 0.409.00.80
12.0
bal Fe
Cu <=0.75; bal Fe
Se 0.2-0.35; bal Fe
485
205
25
bal Fe
485
205
25
UNS numbers and US grades are provided as a means of cross referencing chemically similar alloys. Exchangability is only possible after independent examination of specifications. Tensile properties are minimum or typical as
specified. UTS and YS as MPa. El as %. See Appendix for list of abbreviations used in Notes. * indicates obsolete material.
www.asminternational.org
Notes
Cr
Mn
Mo
Ni
Si
Other
UTS YS El
Hard
Ch18N10SL
Corr res
0.15
max
17-19
2 max
8-12
0.04
0.04
2 max
bal Fe
ZG1Cr18Ni9
0.12
max
17.020.0
0.8-2.0
8.011.0
0.045
max
0.030
max
CSN 422931
422931
Corr res
18-21
1.5 max
8-11
0.045
max
0.04
max
CSN 422932
422932
Corr res
17-20
1.5 max
8-11
CSN 422933
422933
Corr res
0.15
max
0.150.35
0.12
max
17.019.0
1.5 max
9.011.0
0.12
max
8-10
2 max
China
GB 2100(80)
441
196
25
Czech Republic
1-2
0.045
max
0.04
max
bal Fe
France
AFNOR NFA35586 Z10CN189M
Corr res
bal Fe
Germany
TGL 10414
0.1-0.2 18-20
1.5 max
9-11
1.5-2.5 bal Fe
TGL 14394
GS-X10CrNiN197*
Obs
18-20
2 max
6-8
TGL 14415
GSF-X12CrNi189*
Corr res
0.12
max
0.16
max
17-19
1 max
8-10
MSZ 21053(82)
AoX12CrNi189
2 max
8-11
AoX12CrNi189F
0.15
max
0.15
max
17-19
MSZ 21053(82)
17-19
2 max
8-11
GX16CrNi2010
1.5 max
SCS12
0.20
max
18.0021.00
CF-20*
0.2
LH18N9
Corr res
10Ch18N9MLS
Hungary
0.04
max
0.04
max
0.04
max
0.04
max
8-11
0.04
max
0.035
max
2 max
bal Fe
2.00
max
8.0011.00
0.040
max
0.040
max
2.00
max
bal Fe
18-21
1.5
8-11
0.04
0.04
bal Fe
0.15
max
17-19
2 max
8-11
Corr res
0.140.7
17-20
1-1.8
160-230
HB
20L 140-210
HB
450
200
480
205
28
485
205
30
Italy
UNI 3161(83)
Japan
JIS G5121(91)
183 HB
max
Mexico
DGN B-354
Poland
PNH83158(86)
Russia
GOST
0.1-0.2 8-11
0.02
0.02
0.2-1
Cu 0.3; bal Fe
Spain
UNE 36257(74)
AM-X7CrNi20-10
Corr res
1.5 max
8-11
0.040
0.040
2 max
bal Fe
UNE 36257(74)
F.8411*
1.5 max
8-11
0.040
0.040
2 max
bal Fe
ANC3(B)
Corr res
17.020.0
0.202.00
8.5012.0
0.035
max
0.035
max
0.202.00
bal Fe
UNS J92602
0.20
max
Corr res
0.20
max
Noncurrent; Inv cast; 0.25
Corr res
max
Corr res; Solution Q/A 0.20
max
18.021.0
18.021.0
17.0019.00
18.021.0
1.50
max
1.50
max
1.50
0.75
max
max
1.5 max
8.011.0
8.011.0
8.0010.00
8.011.0
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.03
max
0.04
max
2.00
max
2.00
max
2.00
max
2.00
max
bal Fe
UK
BS 3146/2(75)
0.12
max
USA
ACI
CF-20
AMS 5358C(99)*
ASTM
A743/A743M(98)
CF-20
bal Fe
Cu <=0.75; bal Fe
bal Fe
H8A
Corr res
2 max
10-14
0.04
max
0.04
max
2 max
bal Fe
GX16CrNi2414
1.5 max
12-15
0.04
max
0.035
max
2 max
bal Fe
Italy
UNI 3161(83)
UNS numbers and US grades are provided as a means of cross referencing chemically similar alloys. Exchangability is only possible after independent examination of specifications. Tensile properties are minimum or typical as
specified. UTS and YS as MPa. El as %. See Appendix for list of abbreviations used in Notes. * indicates obsolete material.
www.asminternational.org
Notes
Cr
Mn
Mo
Ni
Si
Other
UTS YS El
Hard
SCS17
0.20
max
22.0026.00
2.00
max
12.0015.00
0.040
max
0.040
max
2.00
max
bal Fe
480
205
28
CH-20*
0.2
22-26
1.5
12-15
0.04
0.04
bal Fe
UNS J93402
0.20
max
Corr res
0.20
max
Press ves
0.040.20
Pipe; SA Quen; High- 0.20
temp
max
Corr res; Solution Q/A 0.20
max
22.026.0
22.026.0
22.026.0
22.026.0
22.026.0
1.50
max
00-1.50
12.015.0
12.015.0
12.015.0
12.015.0
12.015.0
0.04
max
0.04
max
0.040
max
0.040
max
0.04
max
0.04
max
0.04
max
0.040
max
0.040
max
0.04
max
2.00
max
2.00
max
2.00
max
2.00
max
2.00
max
bal Fe
bal Fe
485
205
30.0
bal Fe
485
205
30.0
bal Fe
485
205
30
22.025.0
22.025.0
24.026.0
24.026.0
23-25
2.00
max
2.00
max
0.501.50
0.501.50
1.5 max
19.022.0
19.022.0
19.021.0
19.021.0
18-20
0.045
max
0.045
max
0.045
max
0.045
max
0.030
max
0.030
max
0.030
max
0.030
max
1.502.50
1.502.50
0.501.50
0.501.50
1-2.5
bal Fe
bal Fe
1.51-2
bal Fe
450
195
28
bal Fe
450
195
30.0
bal Fe
448
195
30.0
bal Fe
450
195
30
183 HB
max
Mexico
DGN B-354
USA
ACI
CH-20
ASTM A351(94)
CH-20
ASTM A451(97)
CPH20
ASTM
A743/A743M(98)
CH-20
1.50
0.50
max
max
1.50
max
1.5 max
bal Fe
CrNi2520
Heat conducting
DIN 17470(84)
WNr 1.4843
Heating conductor
GX15CrNi25-20
Petrochemical use
WNr 1.4840
Petrochemical use
TGL 10414
0.20
max
0.20
max
0.100.20
0.100.20
0.1-0.2
TGL 14415
0.1-0.2 23-25
1.5 max
18-20
bal Fe
bal Fe
bal Fe
International
ISO DP4991
C68
Corr res
GX16CrNi2521
1.5 max
19-22
0.04
max
0.035
max
2 max
bal Fe
SCS18
0.20
max
23.0027.00
2.00
max
19.0022.00
0.040
max
0.040
max
2.00
max
bal Fe
CK-20*
0.2
23-27
19-22
0.04
0.04
bal Fe
LH25N19S2
Heat res
0.25
max
24-26
0.6 max
17.519.5
0.04
max
0.035
max
2-3
bal Fe
STAS 6855
T25NiCr250X
Corr res
23-27
1.5 max
18-21
1-2.5
bal Fe
STAS 6855(86)
T25NiCr250
0.25
max
0.25
max
23-27
1.5 max
18-21
0.035
max
0.03
max
1-2.5
Pb <=0.15; bal Fe
UNS J94202
0.20
max
Corr res
0.20
max
Press ves
0.040.20
Pipe; SA Quen; High- 0.20
temp
max
Corr res; Solution Q/A 0.20
max
23.027.0
23.027.0
23.027.0
23.027.0
23.027.0
2.00
max
2.00
max
1.50
max
1.50
max
2.00
max
19.022.0
19.022.0
19.022.0
19.022.0
19.022.0
0.04
max
0.04
max
0.040
max
0.040
max
0.04
max
0.04
max
0.04
max
0.040
max
0.040
max
0.04
max
2.00
max
2.00
max
1.75
max
1.75
max
2.00
max
bal Fe
20.022.0
20.022.0
0.03
max
0.03
max
0.03
max
0.03
max
Italy
UNI 3161(83)
Japan
JIS G5121(91)
183 HB
max
Mexico
DGN B-354
Poland
PNH83159(90)
Romania
USA
ACI
CK-20
ASTM A351(94)
CK-20
ASTM A451(97)
CPK20
ASTM
A743/A743M(98)
CK-20
0.50
max
bal Fe
CN-3M
Austenitic Cr-Ni-Mo
CN-3M
Corr res; Cr-Ni-Mo
0.03
max
0.03
max
UNS numbers and US grades are provided as a means of cross referencing chemically similar alloys. Exchangability is only possible after independent examination of specifications. Tensile properties are minimum or typical as
specified. UTS and YS as MPa. El as %. See Appendix for list of abbreviations used in Notes. * indicates obsolete material.
www.asminternational.org
Notes
Cr
Mn
Mo
Ni
Si
Other
UTS YS El
Hard
CN-3M
Corr res
0.03
max
20.022.0
0.03
max
0.03
max
20.022.0
20.022.0
20.022.0
20.022.0
20.022.0
2.00
max
2.00
max
2.00
max
2.00
max
2.00
max
6.0-7.0 23.525.5
6.0-7.0 23.525.5
6.0-7.0 23.525.5
6.0-7.0 23.525.5
6.0023.57.00
25.5
0.040
max
0.040
max
0.040
max
0.040
max
0.040
max
0.010
max
0.010
max
0.10
max
0.010
max
0.010
max
1.00
max
1.00
max
1.00
max
1.00
max
1.00
max
0.08
max
19.021.0
0.045
max
0.03
max
0.08
18-22
1.5
2.5-6
23-27
0.04
0.03
1.2
Cu 1.5-3.5; bal Fe
G-XNiCrMoCuNb2520
WNr 1.4500
0.08
max
0.08
max
19.021.0
19.021.0
2.00
max
2.00
max
2.503.50
2.503.50
24.026.0
24.026.0
0.045
max
0.045
max
0.030
max
0.030
max
1.50
max
1.50
max
Cu 1.50-2.50;
Nb>=8xC; bal Fe
Cu 1.50-2.50;
Nb>=8xC; bal Fe
UNI 3161(83)
19-21.
27-31
18-20
22-25
0.04
max
0.04
max
0.035
max
0.035
max
UNI 3161(83)
0.07
max
0.07
max
435
170
30
550
260
35
550
260
35
390
30
CN-3MN
ACI
CN3MN
ASTM
A743/A743M(98)
ASTM
A744/A744M(98)
CN-3MN
CN-3MN
Corr res
GX8NiCrMoCuNb2520
32
France
AFNOR NFA32056 Z6NCDU252004M
Corr res; SA
Germany
DIN
DIN
Italy
Japan
JIS G5121(91)
SCS23
0.07
max
19.0022.00
2.00
max
2.003.00
27.5030.00
0.040
max
0.040
max
2.00
max
CN-7M*
0.07
19-22
1.5
2-3
27.530.5
0.04
0.04
1.5
bal Fe
GOST
O3ChN28MDT
Corr res
22-25
0.8
2.5-3
26-29
0.8
GOST
O6ChN28MDT
Corr res
22-25
0.8
2.5-3
26-29
0.8
GOST 2246
Sw01Ch23N28M3D3T
Corr res
0.03
max
0.06
max
0.03
max
22-25
0.55
2.5-3
26-29
0.07
max
0.07
max
19.022.0
19.022.0
0.07
max
Corr res
0.07
max
Press ves
0.07
max
Corr res; Solution Q/A 0.07
max
Corr res; severe
0.07
service
max
19-22
183 HB
max
Mexico
DGN B-354
Russia
0.03
0.018
0.55
0.040
max
0.040
max
0.040
max
0.040
max
Spain
UNE 36257(74)
UNE 36257(74)
USA
UNS N08007
ACI
CN-7M
ASTM A351(94)
CN-7M
ASTM
A743/A743M(98)
ASTM
A744/A744M(98)
CN-7M
CN-7M
19-22
19.022.0
19.022.0
19.022.0
27.530.5
1.5 max 2-3
27.530.5
1.50
2.0-3.0 27.5max
30.5
1.50
2.0-3.0 27.5max
30.5
1.50
2.0-3.0 27.5max
30.5
0.04
max
0.040
max
0.04
max
0.04
max
Cu 3.0-4.0; bal Fe
425
170
35.0
Cu 3.0-4.0; bal Fe
425
170
35
Cu 3.0-4.0; bal Fe
425
170
35
UNS numbers and US grades are provided as a means of cross referencing chemically similar alloys. Exchangability is only possible after independent examination of specifications. Tensile properties are minimum or typical as
specified. UTS and YS as MPa. El as %. See Appendix for list of abbreviations used in Notes. * indicates obsolete material.
www.asminternational.org
Notes
Cr
Mn
Mo
Ni
Si
0.08
max
18-22
23-27
0.03
max
0.03
max
19.021.0
19.021.0
1.00
max
1.00
max
2.503.50
2.503.50
24.026.0
24.026.0
0.035
max
0.035
max
0.020
max
0.020
max
1.00
max
1.00
max
2-3
Other
UTS YS El
Hard
Z6NCDU252004M
Corr res
Germany
DIN SEW 410(88)
DIN SEW 410(88)
GX2NiCrMoCuN2520
WNr 1.4536
440- 200
640
440- 200
640
20
Cu 1.5-2.0; bal Fe
485
205
35
Cu 1.5-2.0; bal Fe
485
205
35
490
235
23
20
Romania
STAS 10718(88)
T6CuMoNiCr200
Corr res
0.06
max
18-22
2 max
24-26
0.04
max
0.03
max
UNS J94650
0.07
max
Corr res; Solution Q/A 0.07
max
Corr res; severe
0.07
service
max
18.020.0
18.020.0
18.020.0
1.00
2.5-3.0 22.0max
25.0
1.00
2.5-3.0 22.0max
25.0
1.0 max 2.5-3.0 22.025.0
0.04
max
0.04
max
0.04
max
0.03
max
0.03
max
0.03
max
2.503.50
2.503.50
2.503.50
Cu 1.5-2.0; bal Fe
0.050.15
19.021.0
0.151.50
31.034.0
0.03
max
0.03
max
0.501.50
Nb 0.50-1.50; bal Fe
0.06
max
17.0019.00
11.0014.00
0.045
max
0.030
max
USA
ASTM
A743/A743M(98)
ASTM
A744/A744M(98)
CN-7MS
CN-7MS
CT-15C
Corr res
Cr-Ni-Mo Surgical
Implant 316
422934
Heat res
0.250.45
20.023.0
1.5 max
9.011.0
0.045
max
0.04
max
1.0-2.0 bal Fe
DIN 17465(93)
GX25CrNiSi18-9
Heat res
DIN 17465(93)
GX40CrNiSi22-9
DIN 17465(93)
WNr 1.4825
DIN 17465(93)
WNr 1.4826
0.150.30
0.300.50
0.150.30
0.300.50
17.019.0
21.023.0
17.019.0
21.023.0
1.50
max
1.50
max
1.50
max
1.50
max
8.0010.0
9.0011.0
8.0010.0
9.0011.0
0.035
max
0.035
max
0.035
max
0.035
max
0.030
max
0.030
max
0.030
max
0.030
max
1.002.50
1.002.50
1.002.50
1.002.50
Germany
bal Fe
bal Fe
bal Fe
bal Fe
Italy
UNI 3159
GX30CrNi2010
Heat res
0.2-0.4 18-22
2 max
SCH12
Heat res
0.200.40
2.00
max
0.50
max
8.0012.00
0.040
max
0.040
max
2.00
max
bal Fe
HF*
0.2-0.4 18-23
0.5
8-12
0.04
0.04
bal Fe
UNE 36258(74)
AM-X30CrNi20-10
Heat res
0.2-0.4 18-23
2 max
2 max
bal Fe
UNE 36258(74)
F.8450*
2 max
2 max
bal Fe
302C35
17.022.0
2.00
max
1.50
max
6.0010.0
0.050
max
0.050
max
2.00
max
bal Fe
18.023.0
18.023.0
18-23
2.00
max
2.00
max
2 max
0.50
max
0.50
max
0.5 max
8.012.0
8.012.0
8-12
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
2.00
max
2.00
max
2 max
bal Fe
Japan
JIS G5122(91)
18.0023.00
Mexico
DGN B-355
Spain
UK
BS 3100(91)
USA
UNS J92603
ACI
HF
Heat res
ASTM
A297/A297M(98)
HF
0.200.40
0.200.40
0.2-0.4
bal Fe
bal Fe
UNS numbers and US grades are provided as a means of cross referencing chemically similar alloys. Exchangability is only possible after independent examination of specifications. Tensile properties are minimum or typical as
specified. UTS and YS as MPa. El as %. See Appendix for list of abbreviations used in Notes. * indicates obsolete material.
www.asminternational.org
Notes
Cr
Mn
Mo
0.250.35
0.250.35
19.023.0
19-23
1.50
max
1.50
max
0.50
max
0.50
max
0.50
max
Ni
Si
Other
9.012.0
9-12
0.04
max
0.04
max
0.04
max
0.04
max
0.502.00
0.502.00
bal Fe
UTS YS El
Hard
HF30
bal Fe
ZG40Cr28Ni16
0.200.50
26.030.0
2.00
max
14.018.0
0.040
max
0.040
max
2.00
max
bal Fe
422936
Heat res
0.250.5
24-27
0.045
max
0.04
max
2 max
bal Fe
GX35CrNi2816
Heat res
0.2-0.5 26-30
2 max
SCH18
Heat res
0.200.50
2.00
max
0.50
max
14.0018.00
0.040
max
0.040
max
2.00
max
bal Fe
HI*
0.2-0.5 26-30
0.5
14-18
0.04
0.04
bal Fe
0.200.50
0.200.50
0.2-0.5
26.030.0
26.030.0
26-30
2.00
max
2.00
max
2 max
0.50
max
0.50
max
0.5 max
14.018.0
14.018.0
14-18
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
2.00
max
2.00
max
2 max
bal Fe
0.300.40
0.300.40
26.030.0
26-30
1.50
max
1.50
max
0.50
max
0.50
max
14.018.0
14-18
0.04
max
0.04
max
0.04
max
0.04
max
0.502.00
0.502.00
bal Fe
bal Fe
490
235
490
235
440
230
Czech Republic
CSN 422936
Italy
UNI 3159
Japan
JIS G5122(91)
26.0030.00
Mexico
DGN B-355
USA
UNS J94003
ACI
HI
Heat res
ASTM
A297/A297M(98)
HI
bal Fe
bal Fe
HI35
bal Fe
422952
Heat res
0.30.45
24.027.0
0.045
max
0.04
max
0.751.75
G-X40CrNi2520
Heat res
0.2-0.6 24.028.0
0.04
max
0.04
max
0.300.50
0.300.50
1.50
max
1.50
max
19.021.0
19.021.0
0.035
max
0.035
max
0.030
max
0.030
max
1.002.50
1.002.50
bal Fe
bal Fe
Finland
SFS 393(79)
Germany
DIN 17465(93)
GX40CrNiSi25-20
DIN 17465(93)
WNr 1.4848
24.026.0
24.026.0
bal Fe
Hungary
MSZ 4357
40CrNiSi2520
Heat res
0.2-0.5 24-26
0.5-1.5
19-21
0.04
0.03
1-2.5
GX40CrNi2620
Heat res
0.2-0.6 24-28
2 max
0.04
0.035
HK*
0.5
0.04
0.04
BS 310
310C40
0.3-0.5 24-27
2 max
0.04
0.04
BS 310
310C45
2 max
0.06
0.06
3 max
bal Fe
BS 3100(91)
310C40
310C45
0.300.50
0.50
max
24.027.0
22.027.0
2.00
max
2.00
max
1.50
max
1.50
max
19.022.0
17.022.0
0.040
max
0.050
max
0.040
max
0.050
max
1.50
max
3.00
max
bal Fe
BS 3100(91)
0.200.60
0.200.60
24.028.0
24.028.0
2.00
max
2.00
max
0.50
max
0.50
max
18.022.0
18.022.0
0.04
max
0.04
max
0.04
max
0.04
max
2.00
max
2.00
max
bal Fe
Italy
UNI 3159
Mexico
DGN B-355
18-22
bal Fe
UK
450
bal Fe
USA
UNS J94224
ACI
HK
Heat res
bal Fe
UNS numbers and US grades are provided as a means of cross referencing chemically similar alloys. Exchangability is only possible after independent examination of specifications. Tensile properties are minimum or typical as
specified. UTS and YS as MPa. El as %. See Appendix for list of abbreviations used in Notes. * indicates obsolete material.
www.asminternational.org
Notes
Cr
Mn
Mo
Ni
Si
Other
UTS YS El
Hard
HK
Heat res
0.2-0.6 24-28
2 max
0.04
max
0.04
max
2 max
bal Fe
0.350.45
0.200.35
23.027.0
24.028.0
1.50
max
2.00
max
0.50
max
0.50
max
19.022.0
18.022.0
0.040
max
0.040
max
0.040
max
0.040
max
1.75
max
2.00
max
bal Fe
440
235
0.250.40
0.250.40
23.025.0
23.025.0
1.50
max
1.50
max
23.025.0
23.025.0
0.035
max
0.035
max
0.030
max
0.030
max
0.502.00
0.502.00
230
230
0.250.35
23.0027.00
1.50
max
19.0022.00
0.040
max
0.040
max
1.75
max
bal Fe
440
235
0.250.35
0.250.35
0.250.35
0.250.35
23.027.0
23.027.0
23.027.0
23-27
1.50
max
1.50
max
1.50
max
1.50
max
0.040
max
0.040
max
0.040
max
0.04
max
0.040
max
0.040
max
0.040
max
0.04
max
1.75
max
1.75
max
1.75
max
0.502.00
bal Fe
0.50
max
0.50
max
19.022.0
19.022.0
19.022.0
19-22
450
240
10.0
0.350.45
0.200.35
23.027.0
24.028.0
1.50
max
2.00
max
0.50
max
0.50
max
19.022.0
18.022.0
0.040
max
0.040
max
0.040
max
0.040
max
1.75
max
2.00
max
bal Fe
440
235
0.04
max
0.04
max
0.03
max
0.03
max
1-2.5
bal Fe
500
1-2.5
bal Fe
450
250
440
235
425
240
10.0
450
245
450
245
ZG40Cr25Ni20
JB 4298(86)
ZG3Cr25Ni20Si2
bal Fe
Germany
DIN 17465(93)
GX30CrNiSiNb24-24
DIN 17465(93)
WNr 1.4855
Japan
JIS G5122(91)
SCH21
Heat res
0.50
max
USA
UNS J94203
ACI
HK-30
Heat res
ASTM A351(94)
HK30
Press ves
ASTM A608(98)
HK30
bal Fe
bal Fe
bal Fe
ZG40Cr25Ni20
JB 4298(86)
ZG3Cr25Ni20Si2
MSZ 4357(81)
AoX40CrNiSi2520
0.3-0.5 24-26
0.5-1.5
19-21
MSZ 4357(81)
AoX40CrNiSi2520F
0.3-0.5 24-26
0.5-1.5
19-21
SCH22
Heat res
0.350.45
1.50
max
0.50
max
19.0022.00
0.040
max
0.040
max
1.75
max
bal Fe
UNE 36258(74)
AM-X40CrNi25-20
Heat res
0.2-0.6 24-28
2 max
Nb 1.5; bal Fe
F.8452*
2 max
0.040
max
0.040
max
2 max
UNE 36258(74)
0.040
max
0.040
max
2 max
Nb 1.5; bal Fe
19.022.0
19.022.0
19.022.0
19-22
0.040
max
0.040
max
0.040
max
0.04
max
0.040
max
0.040
max
0.040
max
0.04
max
1.75
max
1.75
max
1.75
max
0.502.00
bal Fe
18.022.0
0.040
max
0.040
max
2.00
max
bal Fe
bal Fe
Hungary
5L
180-230
HB
10L 150-200
HB
Japan
JIS G5122(91)
23.0027.00
Spain
USA
UNS J94204
ACI
HK-40
Heat res
ASTM A351(94)
HK40
Press ves
ASTM A608(98)
HK40
0.350.45
0.350.45
0.350.45
0.350.45
23.027.0
23.027.0
23.027.0
23-27
1.50
max
1.50
max
1.50
max
1.50
max
0.50
max
0.50
max
28.032.0
2.00
max
0.50
max
bal Fe
bal Fe
bal Fe
ZG40Cr30Ni20
0.200.60
10
0.2-0.6 28-32
18-22
0.05
0.05
2.5
bal Fe
SCH23
0.200.60
2.00
max
18.0022.00
0.040
max
0.040
max
2.00
max
bal Fe
India
IS 4522
Japan
JIS G5122(91)
28.0032.00
UNS numbers and US grades are provided as a means of cross referencing chemically similar alloys. Exchangability is only possible after independent examination of specifications. Tensile properties are minimum or typical as
specified. UTS and YS as MPa. El as %. See Appendix for list of abbreviations used in Notes. * indicates obsolete material.
www.asminternational.org
Notes
Cr
Mn
Mo
Ni
Si
Other
UTS YS El
Hard
HL*
0.5
18-22
0.04
0.04
bal Fe
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
2 max
bal Fe
0.5-2
bal Fe
0.5-2
bal Fe
2 max
bal Fe
0.502.00
0.502.00
2
bal Fe
0.04
max
0.04
max
0.04
max
0.04
max
0.502.00
0.502.00
bal Fe
USA
UNS N08604
0.2-0.6 28-32
2 max
UNS N08613
0.2528-32
0.35
0.3528-32
0.45
0.2-0.6 28-32
2 max
0.250.35
0.350.45
0.2-0.6
28.032.0
28.032.0
28-32
1.50
max
1.50
max
2
0.50
max
0.50
max
0.5
18.022.0
18.022.0
18-22
0.250.35
0.350.45
28-32
1.50
max
1.50
max
0.50
max
0.50
max
18-22
1 max
23-28
0.06
max
0.06
max
3 max
bal Fe
UNS N08614
ACI
HL
Heat res
ACI
HL-30
Heat res
ACI
HL-40
Heat res
ASTM
A297/A297M(98)
ASTM A608(98)
HL
Heat res
HL30
ASTM A608(98)
HL40
28-32
18-22
bal Fe
bal Fe
bal Fe
H8F
Heat res
2 max
ZG35Ni24Cr18Si2
0.300.40
1.50
max
23.026.0
0.035
max
0.030
max
1.502.50
bal Fe
11
0.2-0.5 19-23
23-27
0.05
0.05
bal Fe
SCH19
HN*
China
GB 8492(87)
17.020.0
390
195
India
IS 4522
Japan
JIS G5122(91)
19.0023.00
2.00
max
0.50
max
23.0027.00
0.040
max
0.040
max
2.00
max
bal Fe
0.5
23-27
0.04
0.04
bal Fe
bal Fe
390
Mexico
DGN B-355
USA
UNS J94213
ACI
HN
Heat res
ASTM
A297/A297M(98)
HN
Heat res
0.200.50
0.200.50
0.2-0.5
19.023.0
19.023.0
19-23
2.00
max
2.00
max
2 max
0.50
max
0.50
max
0.5 max
23.027.0
23.027.0
23-27
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
2.00
max
2.00
max
2 max
0.350.45
0.350.45
19.023.0
19-23
1.50
max
1.50
max
0.50
max
0.50
max
23.027.0
23-27
0.04
max
0.04
max
0.04
max
0.04
max
0.502.00
0.502.00
bal Fe
0.350.75
24.028.0
2.00
max
33.037.0
0.040
max
0.040
max
2.00
max
bal Fe
440
235
0.300.50
0.300.50
24.026.0
24.026.0
1.50
max
1.50
max
34.036.0
34.036.0
0.035
max
0.035
max
0.030
max
0.030
max
1.002.50
1.002.50
bal Fe
440
230
bal Fe
440
230
0.04
max
0.04
max
0.03
max
0.03
max
1-2.5
bal Fe
500
1-2.5
bal Fe
450
bal Fe
bal Fe
HN40
bal Fe
ZG45Ni35Cr26
Germany
DIN 17465(93)
GX40NiCrSi35-25
DIN 17465(93)
WNr 1.4857
Hungary
MSZ 4357(81)
AoX40NiCrSi3525
0.3-0.5 24-26
0.5-1.5
33-36
MSZ 4357(81)
AoX40NiCrSi3525F
Heat res; SA
0.3-0.5 24-26
0.5-1.5
33-36
5L
250
180-230
HB
10L 150-200
HB
UNS numbers and US grades are provided as a means of cross referencing chemically similar alloys. Exchangability is only possible after independent examination of specifications. Tensile properties are minimum or typical as
specified. UTS and YS as MPa. El as %. See Appendix for list of abbreviations used in Notes. * indicates obsolete material.
www.asminternational.org
Notes
Cr
Mn
Mo
Ni
Si
Other
0.04
0.035
0.040
max
0.040
max
2.00
max
bal Fe
bal Fe
UTS YS El
Hard
GX50NiCr3525
0.3-0.7 23-27
2 max
SCS24
0.350.75
24.0028.00
2.00
max
HP*
24-28
2 max
0.04
0.04
0.350.75
0.350.75
24-28
2 max
2 max
0.04
max
0.04
max
24-28
0.04
max
0.04
max
0.200.35
13.017.0
2.00
max
33.037.0
0.040
max
0.040
max
2.50
max
0.300.50
0.300.50
17.019.0
17.019.0
1.50
max
1.50
max
36.039.0
36.039.0
0.035
max
0.035
max
0.030
max
0.030
max
0.350.75
0.250.35
13-17
33-37
0.05
13-17
0.5
33-37
2 max
Japan
JIS G5122(91)
33.0037.00
440
235
bal Fe
440
195
13
1.002.50
1.002.50
bal Fe
400
230
bal Fe
440
230
0.04
2.5
bal Fe
0.04
0.04
2.5
bal Fe
0.04
0.035
Mexico
DGN B-355
USA
UNS N08705
ASTM
A297/A297M(98)
HP
ZG30Ni35Cr15
Germany
DIN 17465(93)
GX40NiCrSi38-18
DIN 17465(93)
WNr 1.4865
India
IS 4522
120
IS 7806
12
GX50NiCr3919
Heat res
JIS G5122(91)
SCH15
2.00
max
2.00
max
0.50
max
0.50
max
33.0037.00
33.0037.00
0.040
max
0.040
max
0.040
max
0.040
max
2.50
max
2.50
max
440
SCH16
15.0019.00
13.0017.00
bal Fe
JIS G5122(91)
bal Fe
440
HT*
0.350.75
13-17
0.5
33-37
0.04
0.04
2.5
bal Fe
UNE 36258(74)
AM-X55NiCr35--15
Heat res
12-17
2 max
F.8453*
see AM-X55NiCr35-15
12-17
2 max
0.040
max
0.040
max
0.040
max
0.040
max
UNE 36258(74)
0.350.75
0.350.75
330C11
old En4238(H1C)
0.350.55
13.017.0
2.00
max
1.50
max
33.037.0
0.040
max
0.040
max
1.50
max
0.350.75
0.250.35
0.350.75
0.350.75
0.250.35
0.350.75
0.250.35
0.400.60
13-17
2 max
33-37
2 max
15.019.0
15.019.0
13.017.0
15-19
2.00
max
2.00
max
2.00
max
2 max
33.037.0
0.5 max 33.037.0
0.50
33.0max
37.0
0.5 max 33-37
13.017.0
15-19
2.00
max
1.50
max
0.50
max
0.50
max
0.04
max
0.04
max
0.04
max
0.04
max
0.040
max
0.04
max
0.040
max
0.04
max
13-17
0.04
max
0.04
max
0.04
max
0.04
max
0.040
max
0.04
max
0.040
max
0.04
max
Italy
UNI 3159
0.3-0.7 17-21
Japan
4
195
13
Mexico
DGN B-355
Spain
UK
BS 3100(91)
bal Fe
450
USA
UNS N08002
UNS N08030
ACI
HT
Heat res
ACI
HT
Heat res
ACI
HT-30
Heat res
ASTM
A297/A297M(98)
ASTM A351(94)
HT
HT30
Press ves
ASTM A608(98)
HT50
33.037.0
33-37
bal Fe
2.50
max
0.502.00
bal Fe
bal Fe
bal Fe
bal Fe
450
195
15.0
bal Fe
UNS numbers and US grades are provided as a means of cross referencing chemically similar alloys. Exchangability is only possible after independent examination of specifications. Tensile properties are minimum or typical as
specified. UTS and YS as MPa. El as %. See Appendix for list of abbreviations used in Notes. * indicates obsolete material.
www.asminternational.org
Notes
Cr
Mn
Mo
Ni
Si
15-25
2 max
1 max
36-46
0.06
max
0.06
max
3 max
Other
UTS YS El
Hard
H8H
Heat res
0.75
max
bal Fe
422955
Heat res
0.2-0.6 20.022.0
1.5 max
37.040.0
0.045
max
0.04
max
1.0-2.0 bal Fe
MSZ 4357(81)
AoX40NiCrSi3717
0.3-0.5 16-18
0.5-1.5
36-39
bal Fe
450
AoX40NiCrSi3717F
Heat res; SA
0.3-0.5 16-18
0.5-1.5
36-39
0.03
max
0.03
max
1-2.5
MSZ 4357(81)
0.04
max
0.04
max
1-2.5
bal Fe
450
IS4522
0.350.75
37-41
0.05
0.05
2.5
bal Fe
GX50NiCr3919
0.3-0.7 17-21
2 max
0.04
0.035
SCH20
17.0021.00
2.00
max
0.50
max
37.0041.00
0.040
max
0.040
max
2.50
max
bal Fe
HU*
0.350.75
17-21
0.5
37-41
0.04
0.04
2.5
bal Fe
T35CrNi370
0.2-0.5 16-20
1.5 max
35-39
0.035
max
0.03
max
1-2.5
Pb <=0.15; bal Fe
BS 3100(91)
331C40
old En4238(H2C)
331C60
old En1648H2
1.50
max
1.50
max
0.040
max
0.050
max
ANC5(B)
Corr res
37.041.0
36.046.0
36.046.0
0.040
max
0.050
max
BS 3146/2(75)
2.00
max
2.00
max
0.202.00
1.50
max
3.00
max
0.203.00
bal Fe
BS 3100(91)
0.350.55
0.75
max
0.50
max
0.3517-21
0.75
0.4-0.6 17-21
2 max
0.350.75
0.400.60
0.350.75
0.400.60
17-21
2 max
17.021.0
17-21
1.50
max
2 max
0.50
37.0max
41.0
0.5 max 37-41
17-21
1.50
max
0.50
max
37-41
10-14
0.5
0.3510-14
0.75
0.4-0.6 10-14
2 max
0.350.75
0.350.75
0.400.60
10-14
2 max
10-14
2 max
10-14
1.50
max
0.50
max
58-62
15-19
0.5
64-66
Czech Republic
CSN 422955
Hungary
6L
250
180-230
HB
10L 150-200
HB
India
IS 4522
17-21
Italy
UNI 3159(83)
Japan
JIS G5122(91)
390
Mexico
DGN B-355
Romania
STAS 6855(86)
UK
17.021.0
15.025.0
15.025.0
450
bal Fe
bal Fe
USA
UNS N08004
UNS N08005
ACI
HU
Heat res
ACI
HU-50
Heat res
ASTM
A297/A297M(98)
ASTM A608(98)
HU
HU50
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
58-62
0.04
bal Fe
bal Fe
0.04
2.5
bal Fe
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
0.04
HW*
USA
UNS N08001
UNS N08006
ACI
HW
Heat res
ASTM
A297/A297M(98)
ASTM A608(98)
HW
HW50
0.5-2
bal Fe
bal Fe
2.5
bal Fe
HX*
UNS numbers and US grades are provided as a means of cross referencing chemically similar alloys. Exchangability is only possible after independent examination of specifications. Tensile properties are minimum or typical as
specified. UTS and YS as MPa. El as %. See Appendix for list of abbreviations used in Notes. * indicates obsolete material.
www.asminternational.org
Notes
Cr
Mn
Mo
Ni
Si
Other
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.04
max
0.05
max
0.05
max
0.05
max
0.05
max
1.50
bal Fe
max
1.5 max bal Fe
0.04
max
0.035
max
0.025
max
0.04
max
0.04
max
0.035
max
0.04
max
0.04
max
0.04
max
0.035
max
0.04
max
0.025
max
UTS YS El
Hard
0.350.75
0.350.75
0.350.75
0.400.60
15-19
2 max
15-19
2 max
15-19
2 max
15-19
1.50
max
0.50
max
0.150.30
Obs; Heat res; as cast 0.150.3
17.0020.00
17-20
1.50
0.50
8.00max
max
11.00
1.5 max 0.5 max 8-11
ACI
HX
Heat res
ASTM
A297/A297M(98)
ASTM A608(98)
HX
HX50
64-68
bal Fe
I*
422931
Corr res
CSN 422938
422938
Corr res
CSN 422939
422939
Corr res
CSN 422941
422941
Corr res
CSN 422942
422942
Corr res
CSN 422943
422943
Corr res
CSN 422944
422944
Corr res
CSN 422950
422950
Corr res
CSN 422951
422951
Corr res
CSN 422953
422953
Corr res
CSN 422956
422956
Corr res
CSN 422957
422957
Corr res
CSN 422958
422958
PNH83158(86)
0.15
max
0.12
max
0.070.12
0.050.15
0.2 max
18.021.0
20.022.0
15.017.0
17.019.0
18.020.0
0.12
20.0max
22.0
0.3526.00.6
28.5
0.3-0.4 23.025.0
0.2-0.3 20.022.0
0.12
20.0max
22.0
0.2 max 20.022.0
0.0715.00.12
17.0
1.5 max
Corr res
L0H18N9M
Corr res
2 max
PNH83158(86)
LH16N5G6
Corr res
0.07
17-19
max
0.2 max 15-17
PNH83158(86)
LH17N37S2G
Corr res
0.2-0.5 15-19
1.5 max
PNH83158(86)
LH17N8G
Corr res
LH18N10M2
Corr res
16.518.5
17-19
1.5 max
PNH83158(86)
2 max
2-2.5
PNH83158(86)
LH18N10M2T
Corr res
17-19
2 max
2-2.5
PNH83158(86)
LH18N9T
Corr res
17-19
2 max
PNH83159(90)
LH19N14
Heat res
18-20
1 max
PNH83159(90)
LH23N18G
Heat res
0.25
max
0.15
max
0.15
max
0.15
max
0.25
max
0.25
max
22-24
1.5 max
10Ch18N10T
Corr res
2.0 max
0.8-1.5 0.4-0.8
1.5 max 2.0-2.5
1.5 max 2.0-2.5
2.0 max 1.8-2.2
1.0 max
0.5 max
0.5 max
2.0 max
1.0 max 4.8-5.5
0.8-1.5 0.4-0.8
8.00.045
11.0
max
4.5-6.0 0.045
max
11.00.03
13.0
max
9.00.045
11.0
max
9.00.045
11.0
max
4.5-6.0 0.045
max
8.00.045
10.0
max
20.00.04
22.0
max
37.00.04
40.0
max
4.5-6.0 0.045
max
37.00.045
40.0
max
11.00.03
13.0
max
0.04
max
0.035
max
Poland
0.5 max 8-11
6-7
0.035
max
4.5-5.5 0.05
max
37-39 0.035
max
7.5-8.5 0.04
max
9-11
0.035
max
9-11
0.035
max
8-11
0.035
max
13-15 0.04
max
16.50.04
18.5
max
0.035
max
0.035
max
0.035
max
0.035
max
0.035
max
0.035
max
0.035
max
0.035
max
0.035
max
10.011.0
0.02
max
2 max
bal Fe
1-2
bal Fe
1-2.5
bal Fe
bal Fe
2 max
Russia
GOST
1.0-2.0 0.15
max
0.035
max
UNS numbers and US grades are provided as a means of cross referencing chemically similar alloys. Exchangability is only possible after independent examination of specifications. Tensile properties are minimum or typical as
specified. UTS and YS as MPa. El as %. See Appendix for list of abbreviations used in Notes. * indicates obsolete material.
www.asminternational.org
Notes
Cr
Mn
Mo
Ni
Si
Other
UTS YS El
Hard
10Ch18N11BL
Corr res
GOST 977
10Ch18N3G3D2L
Corr res
BS 3100(91)
311C11
old En1648G
BS 3100(91)
330C12
BS 3100(91)
332C11
BS 3100(91)
332C13
BS 3100(91)
332C15
BS 3100(91)
334C11
old En1648(K)
ASTM A351(94)
CT-15C
Press ves
ASTM A451(97)
CPE20N
ASTM
A743/A743M(98)
CK-35MN
1.0-2.0 0.15
max
2.3-3.0 0.15
max
8.00.035
12.0
max
3.0-3.5 0.03
max
0.03
max
0.03
max
0.50
max
0.75
max
0.07
max
0.04
max
0.08
max
0.75
max
17.023.0
13.020.0
19.022.0
24.526.5
21.027.0
10.020.0
2.00
max
2.00
max
1.50
max
1.00
max
1.50
max
2.00
max
1.50
max
1.50
max
2.003.00
1.752.25
1.753.00
1.50
max
23.028.0
30.040.0
27.530.5
4.756.00
4.007.00
55.065.0
0.050
max
0.050
max
0.040
max
0.040
max
0.040
max
0.050
max
0.050
max
0.050
max
0.040
max
0.040
max
0.040
max
0.050
max
3.00
max
3.00
max
1.50
max
1.00
max
1.50
max
3.00
max
bal Fe
19.021.0
23.026.0
22.024.0
0.151.50
1.50
max
2.00
max
31.034.0
8.011.0
6.0-6.8 20.022.0
0.03
max
0.040
max
0.035
max
0.03
max
0.040
max
0.020
max
1.50
max
1.50
max
1.00
max
170
20.0
bal Fe
550
275
30.0
570
280
35
UK
bal Fe
Cu 3.00-4.00; bal Fe 425
34
16
N 0.10-0.25; bal Fe
30
640
bal Fe
USA
0.050.15
Pipe; SA Quen; High- 0.20
temp
max
Corr res
0.035
max
UNS numbers and US grades are provided as a means of cross referencing chemically similar alloys. Exchangability is only possible after independent examination of specifications. Tensile properties are minimum or typical as
specified. UTS and YS as MPa. El as %. See Appendix for list of abbreviations used in Notes. * indicates obsolete material.
Product code
#06814G
Email CustomerService@asminternational.org
www.ameritech.co.uk
Neutrino Inc.
In Japan Takahashi Bldg., 44-3 Fuda 1-chome, Chofu-Shi, Tokyo 182 Japan
Telephone: 81 (0) 424 84 5550
Terms of Use. This publication is being made available in PDF format as a benefit to members and
customers of ASM International. You may download and print a copy of this publication for your
personal use only. Other use and distribution is prohibited without the express written permission of
ASM International.
No warranties, express or implied, including, without limitation, warranties of merchantability or
fitness for a particular purpose, are given in connection with this publication. Although this
information is believed to be accurate by ASM, ASM cannot guarantee that favorable results will be
obtained from the use of this publication alone. This publication is intended for use by persons having
technical skill, at their sole discretion and risk. Since the conditions of product or material use are
outside of ASM's control, ASM assumes no liability or obligation in connection with any use of this
information. As with any material, evaluation of the material under end-use conditions prior to
specification is essential. Therefore, specific testing under actual conditions is recommended.
Nothing contained in this publication shall be construed as a grant of any right of manufacture, sale,
use, or reproduction, in connection with any method, process, apparatus, product, composition, or
system, whether or not covered by letters patent, copyright, or trademark, and nothing contained in this
publication shall be construed as a defense against any alleged infringement of letters patent,
copyright, or trademark, or as a defense against liability for such infringement.