Compressive
Specimen Testing L/D Cross- Max.Load, Corr. Strength,Mpa
Age Diameter Length Remark
No. Date ratio sectional Area kN Factor
Unit Average
20230420-S01-1 93.00 167.40 1.80 6792.91 122.60 1.00 18.0
20230420-S01-2 3d 23/04/2023 93.40 173.40 1.86 6851.47 130.81 1.00 19.1 19.0 Standard-Cured
20230420-S02-2 8d 28/04/2023 93.50 171.30 1.83 6866.15 252.30 1.00 36.7 31.2 Standard-Cured
20230420-S03-2 28d 18/05/2023 94.10 172.28 1.83 6954.55 369.53 1.00 53.1 53.5 Standard-Cured
Remark: The data marked by * is out of the precision range and shall be abandoned.
The compressive strength of shotcrete specimens are 53.5MPa@28days which reached 267% of design grade strength and conforms to requirements of
Coclusion:
project.