TO WHOM IT MAY CONCERN Certificate of Sampling and Analysis
‘We ave examined th samples) of
and epot he folowing te he result
Date : 08 October 2018
Our ref. : 1809754RUS UL
Material Coal
Ex My “GOOD HOPE MAX"
Lot : Average
Weight 57’ 000.000 mt
Port Ust-Luga, Russia
Sampling date 04 - 06 October 2018
We, the undersigned
ces R.S.C., confirm to have attended the loading and
h was loaded on board of the vessel "GOOD HOPE MAX” on 04
rt of Ust-Luga,
= 06 Gctobar 2018 at the
AMPLIN
pling Of coal was carried out during all loading in accordance with I.8.0, Standards.
ANALYSTS
‘TOTAL MoreTURE 1 10.56 8 ASTM D 3302
INHERENT MOTSTURE : 3156 8 ASTM D 3173
ASH IN DRY 14.324 asTM 3174
ASH IN ATR DR a3slai ¥
ASH AS RECEIVED el
VOLATILE MATTER DAF 2 30.86 asm 3175
VOLATILE MAPTER TN DRY : 2642 8
VOLATILE MATTER IN AIR DRIED 25.48 &
VOLATILE MATTER AS RECEIVED 23.63 8
ASTM 5865
SALORIFIC VALUE DAF (Qv) + B12 keal/kg 34.26 Ma/kg.
$ CALOI VALUE IN DRY (ov) F 1010 keat/eg 29.38 Ma/kg
CALORIFIC VALUE IN AIR DRIED (ov) : 6760 keal/eg 28.30 MI/kgy
CALORIFIC VALUE AS RECEIVED (Qv) 5 6270 keal/eg 26.25 MI/kg
NEY CALORIFIC VALUE AS RECEIVED (Op) + 6017 keal/kg 25.19 M/s,
SULPHUR DAF : 0.48 & ASTM 4239
SULPHUR IN DRY oan 8
SULPHUR IN AIR DRIED O40 8
SULPHUR AS RECEIVED : 0.37 &
:XED CARBON DAF t wz 8 ASTM 3172
FIXED CARBON IN DRY 59.3 4
PIXED CARBON IN AIR DRIED 57.2 8
FIXED CARBON AS RECEIVED 5310 4CHLORINE DAF 0.005
CHLORINE IN DRY 0.008
CHLORINE IN AIR DRIED 0.008
CHLORINE AS RECEIVED 0.008
FLUORINE DAF 131
FLUORINE IN DRY Fer}
FLUORINE IN AIR DRIED aoe
FLUORINE AS RECEIVED 200
H.G.T, at 3.04 & residual moisture 63
ULTIMATE AKALISYS
‘CAREON DAF : 85.
CARBON IN DRY to ass
CARBON IN AIR DRIED 70.3
CARBON AS RECEIVED 68.2
HYDROGEN DAF 4.87
HYDROGEN IN DRY re
HYDROGEN IN AIK DRIED 4.02
HYDROGEN AS RECEIVED 3173
‘OPAL HYDROGEN AS RECEIVED palo
(ENCLUDING MOISTURE. HYDROGEN)
NETROGEN DAF 1 aah
NEPROCEN TN DRY 1198
NETROGEN IN ATR DRIED ast
NITROGEN AS RECEIVED Geese]
OXIGEN DAF re ees
OKIGEN IN DRY 6.22
OKIGEN IN AIR DRIED + 6.00
OKIGEN AS RECEIVED 5156
‘ASH FUSION TEMPERATURE IN REDUCING ATMOSPHERE
INITIAL DEFORMATION 1270
SOFTENING i310
HEMISPHERICAL 1360
FLUID yai0
ASH FUSION TEMPERATURE IN OXIDIZING ATMOSPHERE
INETIAL DEFORMATION 1330
SOFTENING 3380
REMESPHERICAL 1410
FLUID 2450
(CARBON DIOXIDE EMISSION FACTOR 94.9
SILICON DIOXIDE
ALUMINIUM OXIDE
IRON OXIDE
(CALCIUM OXIDE
MAGHESTUM OXIDE
SODIUM OXIDE
POTASSIUM OXIDE
MANGANESE DIOXIDE
PHOSPHORUS PENTOXIDE
SULPHUR TRICKIOE
OTHERS
°c
°c
°c
°c
°c
°c
ec
°c
602/75
Page 2
4208
a76a
408
ASTM D 5373
ast D 5373
ASTM D 5373
ASTM D 3160
ASTM D 1857
1857
2003/87/zc
ASH MINERAL ANALYSIS ASTM D 6349
52.0
25.5
6.76
4.70
1180
iis
173
o.ae
0195
0.88
2170
0.55
100.0
‘
8
8
’
.
‘
8
8
‘
8
8
8
‘
nom D so1sSIZING TEST
+ 50 mn
Sizing test was performed on square
aperture sieves
acmt b
snap
Page 3