Professional Documents
Culture Documents
AGC - 2275 Materials Properties Data Book - 1A Nickel
AGC - 2275 Materials Properties Data Book - 1A Nickel
VOLUME 1-A
CLASSIFICATION CATEGORY
UNCLASSIFIED
ii
DISCLAIMER
15 JULY 1970
FOREWORD
This Data Book was p r e p a r e d in p a r t i a l fulfillment of Contract SNP-1 of the Space Nuclear
Propulsion Office, a joint office of the National Aeronautics and Space Administration and the
Atomic Energy C o m m i s s i o n , with the Aerojet Nuclear Systems Company. Guidance of the
work w a s the responsibility of the Cleveland Extension of SNPO.
NHO
•UCLEM iggBQirEiitTiiii
•NERVA
IPROGRAM MATERIALS DATA BOOK PREFACE
This M a t e r i a l s P r o p e r t i e s Data Book has been previously established, and continues in effect,
a s the basic design c r i t e r i o n for m a t e r i a l s usage within the NERVA P r o g r a m , subject to i n t e r -
pretation or extrapolation by the Aerojet Nuclear Systems Company, M a t e r i a l s and P r o c e s s e s
Section.
Submitted: Approved:
e^^^
C . W. Funk, Manager
M a t e r i a l s and P r o c e s s e s Section
v^c^r:^-^. - ^
I. L . O d g e r s , Manager Leepei
Engineering Department Vice P r e s i d e n t and
Technical D i r e c t o r
Aerojet Nuclear Systems Company
PAGE iv NHO
aUCLEtl IIOljn»EII*TII>ll
•X] NERVA TABLE OF
A. P R O G R A M MATERIALS DATA BOOK CONTENTS
DATE
15 JULY 1970
VOLUME 1
SUPERSEDES 15 „ftR 1970
VOLUME 1
INTRODUCTION
Page Page
A. GENERAL 3 B. LIST OF REFERENCES 21
1. O r g anization 4 Reference P r e s e n t a t i o n 22
2. Data P r e s e n t a t i o n 6 1970 23
1969 25
a. Adjustment of Data 6 1968 27
1967 29
b. Identification of P r i m a r y 6 1966 32
Strength P r o p e r t i e s 1965 36
1964 41
c. C a t e g o r i e s of P r i m a r y 7 1963 46
Strength P r o p e r t i e s 1962 50
1961 54
d. Design P r o p e r t i e s 8 I960 56
1959 59
e. Statistical Analysis of 9 1958 61
M a t e r i a l T e s t Data 1957 62
1956 63
f. Symbology 10 1955 64
1954 65
3. Bearing P r o p e r t i e s 12 1953 66
1952 66
4. Modulus of E l a s t i c i t y 12 1951 67
1950 67
5. T h e r m a l E m i s s i v i t y and Emittance 13 1949 68
1948 68
6. Goodman D i a g r a m s 14 1947 69
1946 69
7. Appendices 15 1939 70
1938 70
8. Data Sources 15
PAGE V N H O
HUCLEia BOOMoPEIItTIOIIS
.NERVA TABLE OF
IPROGRAM MATERIALS DATA BOOK CONTENTS
VOLUME J,
MATERIALS DATA
356 I-A-01 43
A356 I-A-02 51
2014 I-A-20 57
2024 I-A-24 61
2219 I-A-26 71
5083 I-A-52 79
5454 I-A-54 81
5456 I-A-56 83
6061 I-A-61 Vol. 1, P a g e 301
7039 I-A-74 97
7075 I-A-75 107
7079 I-A-77 119
7178 I-A-78 125
PAGE vi NHO
KUCLEAR HoenjoPERATIOIIS
"X] NERVA TABLE OF
i . PROGRAM MATERIALS DATA BOOK CONTENTS
DATE
15 JULY 1970
See Pages 4 and 5 of Introduction for Numerical Code VOLUME 1-A
SUPERSEDES
30 SEPT 1969
VOLUME 1-A
MATERIALS DATA
Solution-Hardening Alloys n-A 169 Molybdenum and Molybdenum Alloys III-A 243
Hastelloy C II-A-13 171 Molybdenum ni-A-10 245
Hastelloy N (INOR-8) n-A-14 181
AISI 680 (Hastelloy X) n-A-15 189 TZM Molybdenum III-A-11 257
Inconel 625 n-A-17 197
Tantalum and Tantalum Alloys ni-B 263
P r e c i p i t a t i o n - H a r d e n i n g Alloys II-B 207
Tantalum ni-B-10 265
AISI683 R e n e ' 41 n-B-10 209
AISI 684 Udimet 500 II-B-11 211* Tungsten and Tungsten Alloys in-C 273
AISI 685 Waspaloy II-B-12 213
AISI 687 Udimet 700 II-B-14 215 Tungsten III-C-10 275
AISI 688 Inconel X-750 II-B-15 217 Tungsten-25 Rhenium n i - C - 2 0 283
Alloy 718 II-B-17 223
Udimet 630 II-B-28 231* IV. OTHER NONFERROUS METALS AND ALLOYS
Code Page
D i s p e r s i o n - H a r d e n i n g Alloys n-c 235
Cobalt Alloys IV-A 289
TD Nickel n-c-10 237
AISI 670 Cobalt Alloy (Haynes 25) IV-A-11 291
*To be published
VOLUME 2
MATERIALS DATA
V. FERROUS ALLOYS
Code Page
Carbon and Low-Alloy Steels V-A 315
AISI 1025 V-A-10 317
AISI 4340 V-A-43 319
Austenitic Stainless Steels V-B 321
PAGE viii
rXlNERVA TABLE OF
L I PROGRAM MATERIALS DATA BOOK CONTENTS
30 SEPT 1969
See Pages 4 and 5 of Introduction for Numerical Code VOLUME 3
SUPERSEDES 30 JUNE 1968
VOLUME J.
MATERIALS DATA
VOLUME _J
MATERIALS DATA
C e r a m i c s ( C e m 2nts) DC-E
N a t i o n a l C a r b o n N o . 14 DC-E-IO 663
DW-30 IX-E-11 665
P-514 IX-E-12 667
*To b e p u b l i s h e d
PAGE X
ClEADROC^OPERATIDNI
NERVA TABLE OF
PROGRAM MATERIALS DATA BOOK CONTENTS
30 SEPT 1969
SUPERSEDES 30 JUNE 1968
See Pages 4 and 5 of introduction for Numerical Code VOLUME 3
VOLUME 3
*To be published
PAGE xl
APPROVED FOR USE IN NERVA FINAL DESIGN
\
230
>
V
220
\ PANCAKE FORCINGS - HEAT TREATMENT " B "
TENSILE STRENGTHS, ALLOY 7 1 8
210
• ••— ULTIMATE TENSILE STRENGTH
i2 5-IN THICK
\ •• • TENSILE YIELD STRENGTH
190
k
N DESIGN VALUES,
~">v
s SEE INTRODUCTION, PAGE 8
160
---- T -°^^" df J K ^ ''TU
--- % 5 3
-423 2 10 13 255 3 33 2 71 246
150 o
-320 2 10 18 236 3 33 1 95 229
<
i < i
1 RT 2 4 18 182 3 33 1 95 175
^TV
140 X o
i i z
-423 2 10 18 188 3 33 2 25 180
^S a
s
-320
RT
2
2
10
4
18
18
161
157
3 33
: 33
2 25
2 25
173
149
130 df - DEGREES FREEDOM
i i
120 at o:
110
100
90
80
70
60
SO
-5 -4 -2 -1 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25
TEMPERATURES IN 100° F
o
OPEBtTIOM
160
T - •y
FORCINGS
^l •«»
80
—J J ^^ am m ^ H • • H
160
1
120
40
- 5 - 4 - 3 - 2 - 1 0 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25
TEMPERATURES IN 100° F
226 NMO
• UCLEAR HDlHoPERtTIOai
NRO AND SNPO CONCURRENCE REQUIRED FOR USE IN NERVA FINAL DESIGN
ALLOY 718 ll-B-17
RAM MATERIALS DATA BOOK NICKEL ALLOY
DATE
15 JULY 1970
SUPERSEDES
BASIC DATA
227 NHO
•UClltR ROlHoPIB«TI0>l
.NERVA ALLOY 718 ll-B-17
IPROGRAM MATERIALS DATA BOOK NICKEL ALLOY 6
180
170
BAR - HEAT TREATMENT " A "
STRESS TO RUPTURE
160 ALLOY 7 1 8
0 6 2 5 - t N DIA * ' ' ' * ' • " • STRESS TO RUPTURE
(Diutux ESTIMATED TREND
150
REF 6 5 - 6 1
140
130
5i
120 \
\ \
110
1 -"V \
lo' HOURS--'
100 1
§g
90
V\
^
1 0 ^ HOURS — '
80 y
^ \
70
10'HOURS - '
\-^ V
60 \ \
•^ \
0~
50
40
I \ ^
1
S \
30 X
1%
i
20
a a.
a .^ i \
i i \
s is
5
10 a z
«s
0
-5 -4 -3 -2 -1 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25
TEMPERATURES IN 100° F
228 NWO
•ocLiAB BoclMnopiaATioas
,.), NERVA ALLOY 718 ll-B-17
MATERIALS DATA BOOK NICKEL ALLOY
L. PROGRAM 7
180
170
BAR - HEAT TREATMENT " A " STRESS TO RUPTURE AND CREEP,
ALLOY 7 1 8
160
--""•STRESS TO RUPTURE
0 625-IN DIA
- ^ ^ ^ ^ - STRESS TO 1 % CREEP
150
REF 6 5 - 6 1
140
• -1
» 1
130 °F
120
^ *^-'—„^^^^
Ul
a: 110 •v.,^
u
a
z 100
**" "'- ' • ^
-.
'
J
s. \ : v^.
90 **
•"•'•••••-..... J.. h 1
•••••-..
80 '•••I | 1 2 0 0 °F
•»%
• J
> -s^
70
'„^-S
<:: ^_
60 >
•••..,
50 , 1300 °F
I RECOMMENDED MAXIMUM
^- „__
SERVICE TEMPERATURE
NON-RAC lATlON
40 :s
30
" ' ^ te._
20
'•>. 1
""•
10 ': 11400 °F
,. J
0
10-' 10 0 10' 10^ 10 3 10" 10= 10*
TIME IN HOURS
229 NWO
aUClEAR ROlJlHoPERATIOaS
ALLOY 718 ll-B-17
MATERIALS DATA BOOK NICKEL ALLOY 8
STRESS VS STRAIN
AS FUNCTION OF TEMPERATURE
\—"
„>- „'"^ '-^''-REFERS TO ORDINATE SCALE "B"
REF 6 5 - 6 1
.,1'
TEMPERATURES SHOWN ON CURVES
^
/
^ S'iE—
• — ^
/ y "
Z
,/'"''
r •'•>
,.^
^^^ ^.-
A
iV
' /
1; SCALE "B"
/
/ /
/
7
/
1
/ /
iy
/ /
/
?
r /i^
STRAIN, IN./IN.
NWO >stronuclear
aUClEAR ROOnSOPERATIOaS
iboratory
REDUCTION OF AREA REDUCTION OF AREA
PER CENT PER CENT
/
/
// i
/ o
^
r
-J
r
/ r-
0
--J
<3
> CO
1 O'
f ^
1
1
• 0
>
z0
>
m m
T1
;;! >
Z
•D
ia
m CO
lA
z
M
(A
1 RECOMMENDED MAXIMUM SERVICE TEMPERATURE z
RADIATION X
Ic;
X
n m
2
5 a?
H
s ^ o
m
> o
H
1 RECOMMENDED MAXIMUM SERVICE TEMPERATURE
7s
NON-RADIATION
S
m
z09
H
a;
pp -n
5; 1^ i:.
o w -n=
1
J3 ro N> N> g
ss
m
M V-' 3 IPS
O O
•n
SS£ S; m
S3> o
KSS XI _i
§"S od
Ji 5 5 " S o
'm
'^ n z
^ 1-. ^
»,
ill
S
2 Ji 2 ^ 2 >
K- ro ro CIS
O PO l»
do
O -n
^ >
m
>
^
nHHHMJ
^ ^ • EFFECTS OF IRRADIATION ON ELONGATION OF
FORGING
2 69-2
TIG WELD 1 0 320
- -320 11 7 8 3 9 X 10^^
FORGING
3 69-2
EB WELD 1 0 -320
- -320 13 8 12 0 9 X 10^^
ALL-WELD
-320 69-2
MATERIAL 1 0
- -320 8 3 7 8 9 X 10^^ 2
CW PLUS
4 69-2
AGED ROD 1 0 -320
- -320 9 8 7 5 8 XIO^^
s
FORGING (a) 1 5 130 1050 8 8 7 2 6X10l= 6 4 2 X 10^7 3 70-36 3 7 PPM BORON
1 FORGING 1 0 -423
- -423 14 7 14 6 3 X i o " 3 69-2
m 69-2
FORGING 1 0 320 320 17 17 3 X 10^^
L
230-B NWO
aucLEti aooWOPERHTioas
JO 36
s
"—-„_
28 28
- • ' - _
24 " ^ ' - i ^ 24
^": • ^ , • -
3
i \
20 s
Q.
' \ 20
y-
O ^
<
^^s
1 £
16 <
g
3
Z
i% 16
i
o a
1
S
1
o
o
12 12
^
— "-,^._ - ..OVNAi,
*--"---- -'
'-'—
8
^ • ' • — ,
0
- 5 - 4 - 3 - 2 - 1 0 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25
TEMPERATURES IN 100° F
230-C NMO
RUCIEM RO^BiPIRAIIOai
NRO AND SNPO CONCURRENCE REQUIRED FOR USE IN NERVA FINAL DESIGN
.NERVA ALLOY 718
IPROGRAM
MATERIALS DATA BOOK NICKEL ALLOY
H T A REF 7 0 - 1 6 8 - 3 8 67-44
AND 6 6 6 0
H T B REF 7 0 - 1 AND 6 5 - 1 0 2
i ^
?
s
s E
s
> >1 ESTIMATED MAXIMUM VARIABILITY
0
H T A CURVE -t- 5%
i
< H T B CURVE + lOV.
X X
0
1
i ^^^^^^^
-
1
.11 ' ^
1
^^^^••• t^^^^
r^^^-—*
a; ec
-yy^
,""'
^^^^j'^M •w^^'''^-
^^^^^
,^y/^^
^^•^^>
*SA
REMUS' p^-J„^"'-
.(,.
."<
^^'-^ \ SMOOTHED BEST-FIT CURVE
BASED ON AVAILABLE DATA
/
/
. 5 - 4 - 3 - 2 - 1 0 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25
TEMPERATURES IN 100° F
NHO
lUCLEU loflDDPEIIlTIMI
NRO AND SNPO CONCURRENCE REQUIRED FOR USE IN NERVA FINAL DESIGN
15 JULY 1970
THERMAL CONDUCTIVITY
SUPERSEDES jg jEPT 1967 SPECIFIC HEAT
I B 018
,y"'
'.il!^*
16
^,, . - - -
.,"'•
^ ' • "
y'
r 016
14 014
^//>
^""' , . ' - "
^ , ' y''
12 J ^ ' " .^ 012
r""''
.""'
„^
^ i^'
^ >
>
S-iL
°i
10 , • • " "
^"' "^
J"
^
010
y""
,'^
7^
_. t ^
."^
Si
8 0 08
,'"
SMOOTHED BEST-FIT CURVE
BASED ON AVAILABLE DATA
\ ^''
„^ i
Ui
X
6 y >
1
>g
<
ESTIMATED MAXIMUM VARIABILITY
THERMAL CONDUCTIVITY + 10% 0 06
,/' y s
s
X
<
a;
i
CI
SPECIFIC HEAT + 107.
y 1 a
4 , / 0 04
1 w,^,^. THERMAL CONDUCTIVITY, ALLOY 718
o
/ REF
REF
70-1 69 16 AND 6 8 12 BELOW RT
7 0 - 1 AND 6 8 - 3 8 ABOVE RT
K
^ '^^^^^ SPECIFIC HEAT, ALLOY 718
/
2 CALCULATED BY USE OF FORMULA 0 02
OF LUCKS DEIM AND WEISS
REF 7 0 - 3 2 AND 70-1
/
/
n
-5 -4 -3 - 2 - 1 0 1 3 4 5 6 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25
TEMPERATURES IN 100° F
230-E NMO
aUCLEUR ROqHOPEIKTIOai
IJllVJJI.UL<IJ.IJ.IJIJIIrl:lJJIJ:l:IJ.IIII;IJ.IJ.I:IIL4:IIJIJIJ;llMJIJMB.IJ.4lel.<l
NRO A N D SNPO CONCURRENCE REQUIRED FOR U S E I N N E R V A FINAL DESIGN
15 JULY 1 9 7 0
THERMAL DIFFUSIVITY
SUPERSEDES EMITTANCE
0.90
0.80
HEAT AND THERMAL CONDUCITIVITY
VALUES
0.30 REF. 7 0 - 1
TOTAL HEMISPHERICAL, - 6 0 TO 1 4 0 ° F
TOTAL
0.70
REF. 6 1 - 4 9
-H HEMISPHERICAL r*~
EMI TANCE
1
1
11 1 1 11
'* PLUS CLEANED WITH ALCOHOL, ACETONE AND C C I 4 .
0.60
« (SEE BELOW). ^^
> 0.20 0.50
Ik m .r^x^-"*"
^-'
it ' /•>->"^^
a:
•• «, PLUS PICKLED IN 2% HF + l O y . H N O , SOLUTION "' *->'-^""' THERMAL DIFFUSIVITY, + 15%
0.40
111 ^""'
X
-^f^
„^ ^^/^•*** ^
0^^^^' ^
**•^-"^ g
0.30
ii K
s £ 0.10
* AGED A T 1 4 0 0 F / 1 6 HR IN AIR
- 5 - 4 - 3 - 2 - 1 0 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25
TEMPERATURES IN 100° F
230-F NMO
rnicieo RoiWiii'EiitTiDiis
LJ LU
-k- -^ POISSON'S RATIO, + 10°/.
i v..
S ^-
^ ^
0.28
5
UJ
>g 0.20
<
< < r^^^jr^ DENSITY, ALLOY 7 1 8
i Of
CALCULATED USING THERMAL EXPANSION
Q:
X o DATA, RT VALUE, AND UNIT VOLUME
i CHANGE
S REF. 7 0 - 1
0.27
- 5 - 4 - 3 - 2 - 1 0 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25
TEMPERATURES IN 100° F
230-G
NUCLEAR ROCHroPERATIOIIS
.NERVA ALLOY 718 II-B-17
IPROGRAM MATERIALS DATA BOOK NICKEL ALLOY 16
DATE 15 JULY 1970
ELECTRICAL RESISTIVITY
SUPERSEDES
3U
70
50 rJ^^^
"> 1 ANNEA t-^V.^- ^^,r^^ ^^^^^' ABOVE RT SMOOTHED BEST FIT CURVE
—„. .. ' SAT*NV ^ ry^^^-*" " B A S E D ON AVAILABLE DATA
« E
o u . ^ -
" HEAT J
40
-"- " • < i
a. 0-
[il H
30
o
>^
1 <
< s
X
5
X
1 o
1 i
Q a
20 Z z
o i
^ "^
0
- 5 - 4 - 3 - 2 - 1 0 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25
TEMPERATURES IN 100° F
230-H NMO
NUCLEAR ROUHUPERATIONS