NPK FERTILIZER PLANT MOJOSARI
DUPAN ANUGERAH LESTARI
6
REXLINE SARASWANTI
Toe in
Coma No,
+E] vmoven
® [LF] vmroven asnoren
€ L] voramovn
1 [=] INFORMATION
REVIEWED DOES NOT RELIEVE
CONTRACTORE FORM RESPONSIBILITY
FOR ERROR OR DEVIATIONS FROM
pee) WO NUMBER : WO-264
CONTRACT REQUIREMENTS,
BY: FY DATE : 28 August 2023
Log Date
Out ‘Comm No :
Rev. | Status Description Prepared | Checked | Approved Date
0 Issued For Approval FY CHN
KONSORSIUM DOCUMENT NO. =
VIRRLREI- DAL/QC/VII/2023[boca
RISING BEPECTION READIE coxyvimnoyme-oyrjzaas | 15 uky 2025
ReKhiNe wo
Tee Dopo Avago ost joo So)
Sabict ‘Ring Ring Retry Ory
elorence Drawing 'REI003- M-OWG - 005-006
c0No 2
Project TP Frio Pls Moon Dp Anage a
[fEMoEScRPTION
2, INDIKAS! PATAA PADA SAMBUNGAN LAS
5. INDIKAS ADANYA 2 JENIS KOMPOSSI MATERIAL PADA RDING RING DRYER
b.MEMPERBAI RING RING YANG PATAH DENGAN CARA D WELDING DENGAN MENGUNAKAN METODE YANG SENAR
J. MeNGGANTI MATERIAL RIDING RING ROTARY ORVER YANG PATAA DENGAN YANG BARU.
AGREED OATE FOR COMPLETION OF CORRECTIVE ACTION
user sicnarure
1ESTENATORE
ei Yia Pradana PT REXLINE ENGINEERING INDONESIA)
[VERICATION oF CORRECTIVE ACTION COWPLETEDATE: 15/07/2023
SITE VISIT INSPECTION REPORT NO 004/RE-DaL/svgj/2003
PAGE _:2of2
Terjadikerusakan pada Riding Ring Rotary
Dryer yang mengalamipatah saat Rotary
Dryer beroperasi
Ada indikasi sambungan welding dan yang
patahtepat pada sambungan welding
Pada inikas sarnbungan welding terdapat
bekas cacat welding seperti porosity
aupun sag inclusion.
[Terdapat 2 macam material yang di
|camour untuk material riding ring, material
ay
Feriko Yude Predana|[pect
eee sete cxpmyapconvarmn | 228208
BEARING [ca Pw
Toe PT. Dupo Arogerh Lenton (Najera)
‘subject Fang ing Roary Orr
Referee roving FRE1003-M-DWG- 005-008
SONo EZ
Project. [NP Fenilicr Plant MojnarDupan Angerah Lata
1. Penglasan ing Rng Rotary Ore sis uae
2, Pengelsan Rig Ring Dre ta lckuan Pre Heat
2. Tendopat cat welding sper undercut slag incon, oro, dan sare
ars abutanPre-Heat arera mater yang welding merit Thicknes 100 mm.
carer 2c pests cast welding can hats gern terletu cals kta lakun ep.
|nenetD DATE FOR COMPLETION OF CORRECTIVE ACTION:
Juserstanarure:
[=vALUATION FOR COMPLETION OF CORRECTIVE ACTION
-STGNATORE
@&
erie via Pradana (PT. REXLINE ENGINEERING INDONESIA)
[VERIFICATION OF CORRECTIVE ACTION COMPLETE
ite i ii i ipate: 25/07/2023
SITE VISIT INSPECTION REPORT
No: 002/REI-DAS/sviR/V/2023
PAGE: 2of2
a | EERPPFEH-E-H REMARIGEEEPEEHTV--)
Pengelasan untuk sist ur Riding Ring
Rotary Oryersudah 90%. Sebelum
lakukan pengelasan tidak dilakukan
perlakuan panas (pre-heat) pada material
yang akan dla, Terdapat cacat las
undercut, sag inclusion, porosity, dan
spater.
Untuk sisi dalam Riding Ring Rotary Dryer
belum ciskukan pengelasan dan belum di
bevel
Di bevel terlebih dahulu untuk ruang
Joengelasan. Setelah itu dlakukan Pre-HeatVISITING INSPECTION REPORT
acne Pe
cosmnvaomreroauvayros | 27 ly2023
Reet me mm
Tae Duan Aroperh Lesa cjnat Ste)
Sutiect Fang Rg Ray Ove
Refernce Davin FRETO03- M-OWG- 005-005
sono Ea
reget [Nb Foie Plant Mojoar Dupon Anagerah Lana
[rewosscnrTion
i. Pengelass ding Ring Rotary Dryers ar sudo sles
a. Ado ccat welting dn rack paca pengelasn cng Ring Rotary Orer
5. Proses rept aes welding dan crack dine Ring Rotary Dyer
connective acon
fp Repair lang untuk pan matvilyag crack maupun yang coat welng
J. Hora ernds teen dahuu dan iskutanPre-hest ebelum distulanpengeacan,
[acne DATE FOR COMPLETION OF CORRECTIVE ACTION.
luser sicnarune
[EVACUATION FOR COMPLETION OF CORRECTIVE ACTION
[ac sienaTone
O%
Jecri vid pracana (PT. REXLINE ENGINEERING INGONESA)
jroo
[ESSESESSESEEEEE SESS SESE EESEESSESINSVCe=e-Pc-eecereeeesseeeeeeeteSeLeeeeneerceeereeeEEEE|(Attachment Dokumen Kolom
ke)
(attachment Dokumen Kolom
kea)
permukaan ar sudan a geinda.vibagian|
sarin Riding Ring belum difiishing
arena akan di pasang dabling plat untuk
penguct.
Untuk sisi dalam Ring ing Rotary Dryer
Jsudah dilakukan pengelasan.Terdapat
cacat pengelasan sag Inclusion dan
porosity. Setelahdlakukan pengelasan
teria kerusakan pada material yang clas
(crack yang diakibatkan oleh proses
Jpengelasan.(Gambar 1 dan Gambar 2)
setolah di grinds dlakukan repair
pengelasan pada area yang triad!
kerusaken, Namun sbelum Pengelasan
tidak diakukan Pre-Heat teriebihdabulu
Pengelasan untuk sisi dalam sudahselesai
tingga akcukanfrishing dan
pemasangan dabling plat untuk penguat
sambungan pengelase.
SITE VISIT INSPECTION REPORT
DATE
27/07/2023
No: 003/REI-DAL/SVIR/VI/2023
20f3
cocat las yong teria pada prose pangelasan
harus di gerinda duluseteah itu di Build Up.
Untuk cacat pengelasan sag incusion dan
porosity dakukan penggerindaanterlebih
dahl setelah itu diakukan repair
pengelasan Untuk area material yang teria
kerusokan jga diskukan penggerindaan
teriebin dahul sampal tt terdalam atau
s2mpai kerusakanhilang baru dlakukan
pengelasan. (Gamber 3 dan Gambar 4)
sebelum Pengelasanseharusnya diokukan
Pre-Heat terlebin dahulu untuk menghindart
kerusakan pada material lag.
Diakukan finishing gerinda untuk
|meryesvaixan permukaan material dengan
permukaan sambungan pengelasan
liGamoar 2)arpa
ATTACHMENT DOCUMENT + 008/REL-DAL/SVIR/VI/2023
30f3/
WIEITING NISPECTION REPORT 4 MA/ROMRELDAL/VA/2023 ly 2023,
Reames
Taka FT. Dupan Anvgerh estan ois Ste)
suet ‘Riana Rng Rawr ve
Reference Droving FRETOO8- M-OWNG- O15 066 REI068 =~ DW 005-007
SONe 28
Project ‘NP Fela Pant Moja Dayan Anageah Lata
1. Pengelasan Riding Rng Rotary Dryer sis ar sua sles
2. ado cacat welding dan crack pada pengelasan Rng Rng Rotary Dryer
3. Proves resi caat welding dn rack l Ring Ring Rotary Oryer
‘ORRECTIVE ACTION
separ tng untuk aan mater yang erack maupun yang coat wen
J. Haru i gernds teen dams can elltutonPre-hetSebelumdakutanpengeasn.
Jacnezo DATE FOR COMPLETION OF CORRECTIVE ACTION
[evaLUATION FoR COMPLETION OF CORRECTIVE ACTION
fer Va pracana (FT. REXUINE ENGINEERING INDONESA)
TIFICATION OF CORRECTIVE ACTON COWPLETEFINDING
(attachment Dokumen Kolom
ket)
(attachment Dokumen Kolom
ke2)
(attachment Dokumen Kolom
kea)
setelan me'skukan repair pengelasan
clskukan pemasangan doubling plate
untuk memperkuat pengelasan riding ring
rotary driver. Riding rng di potong setebal
plate dan di gant dengan doubling pate
alu a lakukan pengelasan dengan riding
ring rotary rier. (Gambar 1, Gambar 2,
lcambar 3)
[untuk sis dalam Riding ing Rotary Oryer
Judah cilakukan pengelosan. Terdapat
Jacat pengelasan slag inclusion dan
porosity. Setelah dlakukan pengelasan
teradikerusakan pada material yang di las
crack) yang diakibatkan oleh proses
Jpengelasan.(Gambar 1 dan Gambar 2)
setelah ai gern diakulan repair
Jpengelasan pada atea yang teriadi
kerusakan, Namun sbelum Pengelasan
tidak diakukan Pre-Heat trlebih dahul,
Pengelasan untuk sisi dalam sudah selesai
tinggaldlskukan finishing don
Jpemasangan dabling plat untuk penguat
{sambungan pengelasan.
pare = 28/07/2023,
004/REI-DAL/SviRy/vi/2023
Plate harus i bevel terebih dahulu untuk
Jnembuat rvang pengelasan dengan riding
ring rotary driver. Setelah pengelasan
selsaidilakukan finishing gerinda hina
rata. (Gambar 4, Gambar§)
Urtuk cacat pengelasan slag inclusion dan
porosity dlakukan penggerindaan telebih
[dahuluseteah itu dilakukan repair
Jpengelaean. Untuk area material yang
teradikerusakan juga dilakukan
Joenggerindaan terlebih dahulu samp titik
tercatam atau sampal kerusakan hang baru
[sakukan pengelasan. (Sambar 3 dan
|sambar 4)
[sebelum Pengetasanscharusnya diskukan
Pre-test telebih dahulu untuk menghindst
kerusakan pada material lal
Oviakukan finishing gerinda untuk
Jrenyesuaikan permukaan material dengan
bermukaan sambungan pengelasan.
iGambar 2)DATE: 26/07/2023
ATTACHMENT DOCUMENT No: 004/REI-DAL/S\iR/VII/2023
PAGE: 30f3
Dokumen Kolom ke 1poco a
consyvmoyme-onujzczs | 29 ,uly 2023
VISITING INSPECTION REPORT
REX if ie
Te 7 bapa Aegean Li oS
sti arg nra na OO
Feros Oaning _»REI009- 1 DW O05 RETOGD=M-DWO WOE OAT
SON ma
Pret 1 Fee Fo coer Oopn Fgh a
lata ing Rng Rotary Dryer sil ar sudo sels rising,
doubling pate pada ss yang bin
3, proses pengelosan doubling pate ssl yang ln.
[comnecTiVe ACTON:
>. coubing pte cleaning dn bevel erlbih dah
bs. Diperstan preheat ella dahl
Jaane DATE FOR COMPLETION OF CORRECTIVE ACTION:
Juserstanarure:
[FVALUATION FoR COMPLETION OF CORRECTIVE ACTON
erika Vida bradana (PT. RENLINE ENGINEERING INDONESIA)
TIFICATION OF CORRECTIVE ACTON COMPLETE
cesses ee tasseasesanaaeessssnnesasnssnesssssssstinssisesssese:anstasssssntisIssssiasceeeeienseosessessssssiss |{Attachment Dokumen Kelom
ke2)
(Attachment Dokumen Kolom
ke3)
fan repair pengelasan riding
ring rotary driyer pemasangan doubling,
plate selesa satu ss,
Pengerjan pemasangan doubing pate
pads sis sebalkya dengan di potong
terial dulusesusi dengan teal plate
yang akan oi pasang, (Gambar 1), (Gambar
R)
Doubling pate sudah terpasang dan
selanjutnya diakukan pengelasan untuk
sis sebaicnya
29/07/2023,
(005/REI-DAL/SVIR/VI/2023,
[Sebelortdlakukan pengelasan plate dan
atrial riding rng perlu diekukan finishing
rinda dan di bevel untuk pengelasan
(Gamber 3 dan Gambar 4)
lah colesal proves pengelaran dlakukan
Fishing gerinds untuk visual welding
Jspaye sama dengan materia ing rng.+ 29/07/2023
+ 005/RE-DAL/SVIR/VIl/2023
:30f3,cna
ue/viyRome-DAL/\/2023
VISITING INSPECTION REPORT
REXEINE
Toke FT, Duan Aruger esta (Woisa Ste)
setiect Fig Rng Roary Dvr
'REIOOS- M-DIWG- O05 06, REIOOD- M- DWG- 005 GOs REIOSSM- GWG Dib 006 REGO DWE” 008-008
FRETOOS- > DW. 005-07, REIOOD- M= OW 005-008
a
‘NP Feria Plant Moja Dagon ugerah Lata
1. Pengecean src ing ig yang terasserbiy dengan Ultrasonic Test.
1 penggantian etka eta adorya cata pada material ig ne
|AcreeD parE FoR COMPLETION OF CORRECTIVE ACTION
Juser scnaTune:
VALUATION FOR COMPLETION OF CORRECTIVE ACTION
jacsienarune
Jeerto Wis Pracans (PT. REXUINE ENGINEERING NOONES:A)
Prewans
INERIFICATION OF CORRECTIVE ACTION COMPLETEfoarte saivoznons
SITE VISIT INSPECTION REPORT bo! sonucrewfevmpyn/ancs.
(actachmert Gokamen Klan
|neneriangardmembersian act p89
rasekan tran tet until ro
werhasinvotercopst 5 ti cacat,
eaerencsr esiny edepet 4
[camber 6)
v
|sshuls ssmoakedslaman mm unt
Joengcasan unt renstun os gern.
[dan sears bse santa proses
veal
v
June pres repair ars gain tein
Jrenaarghar/remirsinn coat nade
Jsteral ste gern Sskatan pres
[son seesutnys is shear proses
ea
a cuthing asin Uk erdepat cea
rmnyeurah ke semua matral eet ng
eee pois baher sar
ven
pergcnnn rt ng ory yr Posy
sear 2.70 mm area pera
act pensar yg ero tegoong cles
funk gre epir rar genes
reheat dar seirwany bia clotukonATTACHMENT DOCUMENT
Dokaen Kolom tadATTACHMENT DOCUMENT
lwo
31/07/2023
096
AL/SviR/V/2023
Talon