Screed for Polishing Method

Statement

Step Work Tips

Prepare all side, edges, walls, Bond the isolation using SR 998
column corner for isolation using on the wall. Cut in proper line and
1
isolation PU foam. This should be length and ensure its done
15mm above the final floor level properly

Make sure the sub-base surface


is either compacter WMM over
GSB or PCC within a level If stone soling is done use PCC to
2 tolerance of 5 to 10mm. If level out the surface for
concrete surface then, it should Screeding.
be levelled and free from fragile
surface

The surface should we water Surface should be in surface


3 cured 6 to 7 hours before casting saturated dry state before start of
screed screeding works

Just before start of screeding


screeding apply bonding coat of
Use BS Smartbond 100 and apply
Smartbond 100 diluted with water
4 just when you are about to start
i ration of 1:4. 1 Kg liquid add 4
the concrete
liters water to make 5 liters and
spread it on the surface.

In the mix add VPP Fiber 24mm at


125 gms per bag of cement or
Screed Mix has to be minimum M-
5 900 gms per cum, also add 5kg
25, made only in OPC Cement.
SRA agent to the mix at 5Kg per
cum.

On the installed panel, place the


concrete and make sure needle Flex Screed, Magic Screed or
6 vibrator is used properly when Walk Behind Laser can be used
levelling and screeding the for larger area
flooring

7 For small area screeding has to be


done manually , but ensure levels

Screed for Polishing Method Statement 1


Step Work Tips
are maintained and cross checked
with Laser Guided Levelling
System or experienced mason

Apply dryshake hardener in 2 or Application in 2 layers for 5kg per


three steps. Use minimum 5kg per sqm or more as per requirement.
8
sqm of Dryshake Hardener for Spread evenly with proper
even application application.

When the screed if levelled , For power floating is done and


9 using finishing tools like power the finishing blades are used to
floater and ride on trowel, closed the surface

While Hardener Application start,


apply densifier chemical just
Use BS FloorDense-Lin at 15 Sqm
before application of first layer of
per litre in first time spray, use 15
hardener , then apply second
10 Sqm in second spray and finally
layer of densifier after second
use 15 Sqm per liter in the and
layer of dryshake and finish and
final finishing blade operation
finally apply densifier chemical on
final troweling.

Joint Cutting to be done within 24 Cut with Heavy Duty Diamond


12
to 48 hours. Cutter Machine

Curing to be done for 8 days Using plastic sheet 75% less


13
using plastic sheet. water will be required.

Sealant to be filled after 14 days


14
of last curing days

Grinding and Polishing to start


16 after 28 to 30 days of all works
completed