TESTREPORT

TestReportNumber : DCCD-9149Dated: 08.08.2006

Name& Addressof the Customer of IndiaLtd ,


: M/s CableCorporation
DattapadaRoad,Borivli( (E),Mumbai- 400 066

of IndiaLtd '
Name& Addressof the'Manufacturer: M/s CableCorporation
DattapadaRoad'Borivli( (E)' Mumbai- 400 066

Particularsof samPle tested : 3X 400 sq.mm, 19/33kV, XLPECable


in Red Pen
Conditionof the samPleon receiPt : Verifiedand foundPaperSealand Marking
signedby omkar. A.salunke on the cablewith information.
following
" [ot No.'6468,CableNo.29996,TypeA2XCEFY3 X 400 RMA/
19/33kV (E) ,Length15 metres"
Type : A2XCEFY
Designation :Conductor Material: Aluminum
Size: 400 mm2
Numberof cores: Three
: XLPE
lnsulation
Armour.Galvanised SteelStriP
Outersheath:PVC
'19/33kV
VoltageRating.

S e r i aN
l umber : CableNo.29996,Lot No.6468'DrumNo.6AJ26'16-'14
Numberof SamPlestested :One
Date(s)of Test(s) : 3 0 . 0 6 . 0t6o 0 8 . 0 8 . 0 6
C P R IS a m p l eC o d en o ( s ) . DCCDCABOoSO5ST

Particularsof test conducted : TypeTest


Test in accordancewith
Standard/SPecification /Am | 1988
: As per lS 7098(Part-ll)-1985
Samplingplan : NotApplicable
Customer's requirement :Nil
Deviation if any : Nil

Nameof the witnessingPersons


Customer'srePresentatives : None
Otherthan customer'srepresentatives : N o n e .

Test subcontracted with address


of the laboratorY . Nil
Documents constitutingthis report (in words)
Numberof sheets : Ten + one reportof 3 pages
Numberof osctllogram/s : Twelve(Three Pages)
N u m b e ro f g r a P h s . Nil
Numberof photos :Nil
Numberof testcircuitdiagrams : Nil
:Nil
( -c:c{9r
Lin.suorrinoral
"
Joint Director

R D C C D 9 l 4 qI 2 0 . ) 2 0 0 6
CABLES LABORATORY
D IA GN OS T ICC, ABLES& CAPACITORSDIVISION
C E N T R A LP OW ERRESEARCHINSTITUTE
P . B .N o . 8 0 6 6S, A D A S I V A N A G ASRU B P . O .
P R O FS I RC . V . R A M A NR O A D, B A N G A L O R-E5 6 0O 8 OI,N D I A . NABLAccredited
CPRI Phone' +9'1(0) 80-23604435. Fax : +91 (0) B0- 2360'12'13 Laboratory
Cert.No.T-0010

Sheet 2 of '10
TESTREPORT
TestReportNo.:DCCD-9149 Date:08.08.2006

TESTRESULTS

CONDUCTORRESISTANCE TEST:
Core in Q/Kmat 20" C
Resistance
ldentification Value(Max)
Specified

Red
Yellow 0.07330 0.0778
Blue 0.07440
Conclusion: The specimenmeetsthe requirementsof the specification

I I . T E S T SO N A R M O U R
1 . T e s tf o r d i m e n s i o n s :

a ) T y p e: G a l v a n i s eSdt e e S
l trip
d o m i n a l T h i c k n e :s0s. 8 0 t 1 0 % m m
b ) S o e c i f i eN
c) ObservedNominalThickness: 0.83mm
d) Conclusion: The specimenmeetsthe requirementsof the specification

2. TensileStrengthand Elongationat break :

As oer ReoortNo. INS/M/003/Julv/06-07


Dated22.07.06

3. Mass of Zinc coating:

a ) S p e c r f i evda l u e ( m i n.) 1 1 0 g l m 2
b) Observedvalue '. 318.23glm'
c) Conclusion: The specimenmeetsthe requirementsof the specification

4. Uniformityof Zinc Coating:

a) REQUIREMENT: No red depositsof copperto be observedon the basemetalaftertest.


b) RESULT:No red depositof copperwereobservedon the basemetal afterthe test.
c) Conclusion: The specimenmeetsthe requirementsof the specification

5. WrappingTest :

a) REQUIREMENT: No Breakingor Splitting


to be observedafterwinding
and strarghtening.
b) RESULT:No Breakingor Splittingobservedafterwindingand straightening.
c) Conclusion: The specimenmeetsthe requirementsof the specification

6. AdhesionTest :
a) REQUIREMENT : No cracksor any otherabnormalities
to be observedaftertest.
b) RESULT No cracksor any otherabnormalities wereobserved.
c) Conclusion: The specimenmeetsthe requirementsof the specification
A
,41 ^il \
'il| il 'lt/t I
!t /nt l,fry
,,

lrrrirumurtnffi
T E S TE N G I N E E R
CABLES LABORATORY
D IA GN OS T ICC, ABLES& CAPACITORSDIVISION
C E N T R A LP OW ERRESEARCHINSTITUTE
P.B.No.8066,SADASIVANAGAR SUB P.O
PROF.SIR C.V.RAMAN R O A D, B A N G A L O R-E5 6 0O B OI ,N D I A . NABLAccredited
CPRI P h o n e + 9 ' l ( 0 ) 8 0 - 2 3 6 0 4 4 3 5F,a x : + 9 1 ( 0 ) B 0 - 2 3 6 0 1 2 1 3 Laboratory
N o.T - 001
C er t.

Sheet 3 of 10
TEST REPORT

Test ReportNo.: D C C D - 9 1 4 9 Date:08.08.2006

TEST RESULTS

I I I .T E S T SO N I N S U L A T I O N

OF INSULATION:
1 . T E S TF O RT H I C K N E S S
s t . Core ObservedValuesin mm Soecified Valuesin mm
No ldentrfrcation M i n i m u m Averaoe M i n i m u m Averaqe
1 Red 8.714 8.996
a
z Yellow 8.746 9.013 7.82 B.BO
3. Blue 8.751 8.948
Conclusion: The specimenmeetsthe requirementof the specification

2. TENSILESTRENGTHAND ELONGATION AT BREAK


A . B E F O R EA G E I N G ;
Core ObservedValues SpecifiedValues(Min)
SI ldentification Tensile Elongation Tensilestrength Elongation
No strength At Break(%) N/mm' at Break(%)
N/mm'
I Red 20.93 615.5
a Yellow 2 2 . 4 6 618.5 12.5 200.0
3 Blue 21.10 606.75

B .A G E I N G :
Sample Temperature Duration
D u m b -b e l lS o e c i m e n s 1 3 5t 3 " C 1 6 8H o u r s

C . A F T E RA G E I N G :
Core ObservedValues
S l . N o ldentification TensileStrengthN/mm' at Break (%)
Elongation
1 Red 20.75 606.50
a
Yellow 20.0 589.5
J- Blue 20.31 591.75

D. VARIATIONS OBSERVEDFROM BEFOREAGEINGSAMPLES


Core Observed% Variations Specified% Variations (Max)
bt. ldentification Tensile Elongation Tensile Elongation
No strenqth (%\ At Break (%) Strenoth(%) at Break(%)
1 Red -0.84 1.46
.)
Yellow 1' 1 . 0 3 -4.69 x25 L25
Blue -3.76 -2.+ I

Conclusion: The specimenmeetsthe requirementsof the specification

(Thirumurthy) f.
T E S TE N G I N E E R
CABLES LABORATORY
D IA GN OS T ICC, ABLES& CAPACITORSDIVISION
C E N T R A LP OW ERRESEARCHINSTITUTE
P . B .N o . 8 0 6 6S, A D A S I V A N A G ASR U BP . O .
PROF.SIR C.V.RAMAN R O A D, B A N G A L O R-E5 6 0O 8 OI,N D I A . NABLAccredited
P h o n e: + 9 1 ( 0 ) 8 0 - 2 3 6 0 4 4 3 5F,a x: + 9 1 ( 0 )B 0- 2 3 6 0 1 2 1 3
CPRI Laboratory
Cert.No.T-0010

S h e e t4 o f 1 0
TESTREPORT

Test ReportNo.: DCCD-9149 Date:08.08.2006


TEST RESULTS

3 . WA I b , RA t s S O R PI I O N TEST
I t s , SI : ( G R AV I M E T R I C
Sl.No Core Waterabsorbedin mo/cm'
ldentification Observedvalues Value(Max)
Specified
1 Red 0.012
a
L Yellow 0.012 1.0
Blue 0.01'1
Conclusion: The specimenmeetsthe requirementsof the specification

4. SHRINKAGT EE S T
SlNo Core Shrinkaqe in Percentaqe(%)
ldentification Observedvalues Specified
Value(Max)
1 Red t.oo
2. Yellow 1. 5 8 4.0
3 BIue 1.78
Conclusion: The specimenmeetsthe requirementsof the specification

5" HOT SET TEST:


>t. Core ObservedValues(%) (%)
SpecifiedValues(Max)
N o , ldentification Hotset Permanent
set Hotset Permanent set
Elonqation Elonqation Elonqation Elonoation
1 Red 93.75 0.10
a
Yellow 80.0 0.10
1 75 . 0 15.0
3. Blue t t c 0.125
Conclusion: The specimenmeetsthe requirementsof the specification

IV.TESTSON OUTERSHEATH:
l.THICKNESS:

a ) S o e c i f i eM
d i n i m u m : 3 . 0 0m m
b ) O b s e r v eM d i n i m u m : 3 . 6 8m m
c) Conclusion: The specimenmeetsthe requirementsof the specification

2 . T E N S I L ES T R E N G T H
A N D E L O N G A T I OA
NT B R E A K
A . B E F O R EA G E I N G

a ) S p e c r f r eTde n s i l eS t r e n g t (hM i n ) : 1 2 . 5N / m m 2
E l o n g a t i oant B r e a k( M i n ) . 1 5 0%
b) ObservedTensileStrength '. 14.55N/mm'
Elongation at Break '.296.5%

B.AGEING
a) Sample D u m b - b esl lp e c i m e n s
b )T e m o e r a t u r e . 1 0 0t 2 " C
/ \
c) Duration 168 hours h llt 1
/t{h*1/Yir^4 I
+_-_____-____-L_Ty
( T h i r u m u r t)h\ f
T E S TE N G I N E E R
CABLES LABORATORY
D IA GN OS T ICCABLES
, & CAPACITORSDIVISION
C E N T R A LP OW ERRESEARCHINSTITUTE
P.B.No.8066,SADASIVANAGAR SUB P.O.
PROF.SIR C.V.RAMAN 0 B OI ,N D I A .
R O A D, B A N G A L O R E . 5 6O NABLAccredited
+91 (0) Fax : +9'l (0) B0 - 2360'1213 Laboratory
CPRI Phone' B0-23604435,
. o .T - 0 0 1
C e r tN
Sheet5 of 10
TESTREPORT
Test ReportNo.: DCGD-9149 Date:08.08.2006

TEST RESULTS
C . A F T E RA G E I N G

a ) S p e c i f i eTde n s i l eS t r e n g t (hM i n ) : 1 2 . 5N / m m 2
Elongation at Break(Min) . 150%
'14.86N/mm2
b) ObservedTensileStrength
at Break
Elonoatton 269.5 %

OBSERVEDFROM BEFOREAGEINGSAMPLES
D. VARIATIONS

maximumvariations
a) Specified . )_25%
b) ObservedvariationsTensilestrength + 2 . 1 30 k
at break "'. -9.11%
Elonqation
Conclusion: The specimenmeets the requirements of the specification

3. LOSSOF MASSTEST:

a) Samole :Dumb-bellspecimens
b)Temperature : ' 1 0 01 2 "C
c) Duration : 1 6 8h o u r s
'I
d) Specified lossof mass (Max) ^nln^Z

e) Observedlossof mass : 0.95mg/cm'


f ) C o n c l u s i o n: T h e s p e c i m e nmeetsthe requirementsof the specification

4. SHRINKAGT EE S T
'.4%
a ) S p e c i f i e(dM a x )s h r i n k a gael l o w e d
b ) O b s e r v eS d hrinkage . 1 . 4 0%
c) Conclusion: The specimenmeetsthe requirementsof the specification

5. HOT DEFORMATION TEST


depthof indentation : 50 % (Max)
a) SpecifiedPercentage
b) ObservedPercentage depthof indentation .22.55%
c) Conclusion: The specimenmeetsthe requirementsof the specification

6. HEATSHOCKTEST
a) REQUIREMENT shouldbe observedaftertest
. No Cracksor any otherabnormalities
b) RESULT No Cracksor any otherabnormalitieswereobservedaftertest
c) Conclusion: The specimenmeetsthe requirementsof the specification

7. THERMALSTI\BlL|TYTEST

time
thermalstability
a) Specified : 8 0 m i n u t e s( m i n )
b) Observedthermaistabilitytime : GreaterthanB0 minutes
c) Conclusion: The specimen meetsthe requirementsof the specification ,, ."\
)t u\
( \tw'^lY\1
(Thirumurth{).'
T E S TE N G I N E E R
CABLES LABORATORY
D IA GN OS T ICC, ABLES& CAPACITORSDIVISION
C E N T R A LP OW ERRESEARCHINSTITUTE
U BP . O .
P . B .N O . 8 0 6 6S,A D A S I V A N A G ASR
PROF.SIR C.V.RAMAN R O A D, B A N G A L O R-E5 6 0O 8 OI,N D I A . NABLAccredited
Phone: +91 (0) 80-23604435, Fax : +91 (0) 80 - 23601213 Laboratory
CPRI C e r t .N o .T - 0 0 1 0

S h e e t6 o f 1 0
TEST REPORT
Test ReportNo.: DCCD-9149 Date:08.08.2006

TEST RESULTS

O F I N N E RS H E A T H
8.THICKNESS

d i n i m u m : 0 . 7 0m m
a ) S p e c i f i em
' 1 . 4 6m m
b ) O b s e r v em d inimum :
c) Conclusion: The specimenmeetsthe requirementsof the specification

V. ELECTRICAL TESTS
testswerecarriedout in the orderof sequence.
electrrcal
The following

TEST:
l.PARTIALDISCHARGE

a) Lengthof the sample : 10.50metres


b) Sensitivrty of the detector : 5 PC
c) Methodof connection : Two endsof the cablewereimmersedin oil withhighvoltageapplied
to conductor and othercoresshortedto groundedmetallicshield& armour
d ) M e a s u r i nvgo l t a g e( 1 . 5U o ) : 2 8 . 5k V a c
' 1 . 5U o ( M a x ): 2 0 p C
e ) S p e c r f i eddi s c h a r gme a g n i t u daet
ObservedIlrscharqe Itude
SlNo Core ldentification e a q n i t u dien p C
D i s c h a r qm
1 P o d Less than 5 pC
2. Yellow Less than 5 pC
3. Blue Less than 5 pC
g) Conclusion: The specimenmeetsthe requirementsof the specification

2 . B E N D I N GT E S T

a) Outerdiameterrof cable . 110 mm


b) Diameterof testcylinder : 2200 mm
c) Numberof bendingcycles : Three

TEST
3, PARTIALDISCHARGE

a) Lengthof the sample : 10.50 metres


of the detector
b) Sensitivity : 4 nf-
c) Methodof connection : Two endsof the cablewereimmersedin oil withhighvoltage
appliedto conductor and othercoresshortedto grounded
m e t a l l isch i e l da n da r m o u r
d) Measuring voltage(1 5 Uo) : 28.5kV ac
e a g n i t u daet 1 . 5U o ( M a x ): 2 0 p C
e ) S p e c i f i eddi s c h a r gm
f) ObservedDischargemagnitude

Sl.No Coreldentification Discharqemaqnitude in pC


1 Red Lessthan5 pC
2 Yellow Lessthan5 pC
3 Blue Lessthan5 pC
g) Conclusion: The specimenmeetsthe requirementsof the specification
CABLES LABORATORY
D IA GN OS T ICC, ABLES& CAPACITORSDIVISTON
C E N T R A LP OW ERRESEARCHINSTITUTE
P . B .N o . 8 0 6 6S, A D A S T V A N A GS AURB p . O .
PROF.SIR C.V.RAMAN R O A D, B A N G A L O R-E5 6 0O 8 OI,N D I A . NABLAccredited
CPRI P h o n e: + 9 1 ( 0 ) 8 0 - 2 3 6 0 4 4 3 5F,a x : + 9 . 1( 0 )B 0- 2 3 6 0 1 2 1 3
Laboratory
C e r tN
. o .T - 0 0 1 0
S h e e t7 o f 1 0
TEST REPORT
Test ReportNo.:DCCD-9149 Date:08.08.2006

TEST RESULTS

4. TAN DELTAMEASUREMENT
AS A FUNCTIONOF VOLTAGE

a) Specified tan deltaat Uo(Max) 0.004


b) Specifiedincrement from 0.5 Uo to 2Uo : 0.002(Max)
c ) A m b i e ntte m p e r a t u r e .2goc
d) ObservedV a l u e s :
Core Tcs.t \/nltrno Tan delta Capacitance Incrementof
N o ldentification (kV)ac (AbsValue) inPF Tan Delta
9.5 0.000092
1 Red 19.0 0.00014 2366.0
38.0 0.00022 + 00 0 0 1 3
9.5 0.000096
t Yellow 19.0 0.00018 z+tt.o
38.0 0.00020 +0.000104
9.5 0.000098
3 Blue '19.0
0.00019 2 3 8 0B.
38.0 0.00021 + 0 0 0 0 11 2
e) conclusion : The specimenmeetsthe requirementsof ttrespeciricatr'on

5. TAN DELTAMEASUREMENT AS A FUNCTIONOF TEMPERATURE


a) Temperature 0
of the conductorduringtest : g0 C
b) TestVoltageduringmeasuremenl ' . 2 k Ya c
c) Specified Tan detta(Max) : 0.008
d) ObservedValues:-
S l . N o Core Tan delta Tan delta Capacitancein
ldentificationat 28 oC At 900c Picofarad
1 Red 0.000088 0.000218 2234.7
a
z. Yellow 0.000090 0.000224 2279.3
3 Blue 0.000092 0.000220 zz+o.u
e) conclusion : The specimenmeetsthe requiremenisof ftre specification

6. INSULATIOR
N E S I S T A N CTEE S T
sr. Core ObservedVolumeResistivity SpecifiedVolumeResistivity
No ldentrfication in O-cm rnfi-cm(Min)
at 28 "C at 90 "C OL ZI U at 90 "C
1 Red 1 . 3 1X 1 0 1 6 5 . 6 4X 1 0 1 5
a
Yellow 3 . 4 0X 1 0 1 7 7 . 3 5X 1 0 1 5 '1
x 1014 1 x 1012
3 Blue 4 . g BX 1 0 1 7 7 . 6 6 X ' 1 0 1 5
Conclusion
: Thespecimenmeetsthe requiremffi

7. HEATINGCYCLETEST

a) ConductorTemperature duringHeatingCycle: 1000C


b) Heatingperiodafterattaining
Temperature : 4hours
c) NaturalCoolingPeriod : 4 hours
d) Numberof heatrngcycles . 3 Onlv
(sM 1l
(Thirumurthy
\

T E S TE N G I N E R
CABLES LABORATORY
D IA GN OS T ICC, ABLES& CAPACITORSDIVISION
C E N T R A LP OW ERRESEARCHINSTITUTE
P.B.No.8066,SADASIVANAGAR SUB P.O.
P R O FS I R C . V . R A M A N R O A D B A N G A L O R-E5 6 0O 8 OI,N D I A . NABLAccredited
F,a x: + 9 1( 0 )8 0 - 2 3 6 0 1 231
P h o n e. + 9 1 ( 0 ) B 0 - 2 3 6 0 4 4 3 5
CPRI Laboratory
C e r tN
. o T-0010
S h e e t8 o f 1 0
TEST REPORT
Test ReportNo.: DCCD-9149 Date:08.08.2006

TEST RESULTS

8. TAN DELTAMEASUREMENT AS A FUNCTIONOF VOLTAGE


a) Specrfied tan deltaat Uo(Max) : 0.004
b) Specified increment from 0.5 Uo to 2Uo : 0.0-02 (Max)
c ) A m b i e ntte m o e r a t u r e .27 "C
d) ObservedValues.
-T-a^
Jl. Core Test -l^l+a
I qtt uEtto in Pf
Capacitance lncrement
N o ldentificationVoltage (AbsValue) of
(kV)ac Tan Delta
9.5 0.000098
1 Red 19.0 0.00012 2364.3
38.0 0.00019 +0.000092
9.5 0.00009
a
Yellow 19.0 0.00014 24151
38.0 0.00025 +0.00016
3. Blue 9.5 0.00011
19.0 0.00017 2378 4
38.0 0.00024 +0.000'13
e) Conclusion: The specimenmeetsthe requirementsof the specification

9. PARTIALDISCHARGE TEST
a ) L e n g t ho f t h e s a m p l e : 1 0 . 5 0m e t r e s
' 4 n f
b) Sensitivity of the detector
c) Methodof connection : Two endsof the cablewereimmersedin oil withhighvoltage
appliedto conductor and othercoresshortedto grounded
m e t a l l isch i e l da n d a r m o u r
d) Measuring voltage(1 5 Uo) : 2 8 . 5k V a c
e) Specifieddischargemagnitude at 1 . 5U o ( M a x ): 2 0 p C
f) ObservedD s c h a r q e m a q n r t u d e
Sl.No Core ldentification Discharqe maqnitude in pC
1 Red Lessthan5 pC
a
L Yellow Lessthan5 oC
J. Blue Lessthan5 oC
g) Conclusion: The specimenmeetsthe requirementsof the specification

1 0 .I M P U L S E
WITHSTAND TEST:
Date of Test Temperatureof OtO'un,,oa.,Temperatu re N o . o f
Test Voltage Conductor lmpulses
kV peak DurinqTest(oC) D r vB u l b Wei Bulb
10Positive
2 4 . 0 70 6 170.0 95.0 25.0 23.0 &
1 0N e o a t i v e

The impulsesourcewas connected to the conductor


of the
the particular
core (endsshorted)undertestand the screenconnected to
ground.The conductors of the othertwo coreswhichwere not undertest
wereshortedtoqetherwith screenand connected to qround.

T E S TE N G I N
CABLES LABORATORY
D IA GN OS T ICC, ABLES& CAPACITORSDIVISION
C E N T R A LP OW ERRESEARCHINSTITUTE
P . B .N o . 8 0 6 6S, A D A S I V A N A G ASRU B P . O .
PROF.SIR C.V.RAMAN R O A D, B A N G A L O R-E5 6 0 O 8 OI,N D I A . NABLAccredited
Phone: +91 (0) 80-23604435, Fax : +91 (0) B0- 2360'1213
CPRI Laboratory
C e r tN
. o .T - 0 0 1 0

Sheet9 of 10
T E S TR E P O R T
Test ReportNo.:DCCD-91
49 Date:08.08.2006

TEST RESULTS

Core Polaritv S h o tN u m b e r Number


Oscilloqram TestResult
Red Positive First
Tenth IJJ I Withstood
Negative First
Tenth 1401
Yellow Positive First 1413
Tenth 1419 Withstood
Negative First 1423
Tenth 1428
BIue Positive First IZ+JO

Tenth 1440 Withstood


Negative First 1443
Tenth 1448
( o s c rL L o G R A ME
SN C L O S E D )
Conclusion
: Thespecimenmeetsthe requirements
of the specification

1 1 .H I G HV O L T A G ET E S T

a\
v l
Tocf cnnnontinn Betweentest core and othercores
shortedto groundedshieldand armour
h\ Tact \/nliena 57 kV ac
.\ l..)rrrrtinn nf tacf 4 Hours
^^0 ^
d) AmbientTemperature z v v
e) Lengthof Sample 1 0 . 5 0m e t r e s
Resu
Sl.No. Coreldentification Remarks
Red WITHSTOOD
2 Yellow WITHSTOOD
3 Blue WITHSTOOD
g) Conclusion: The specimenmeetsthe requirementsof the specification

1 2 .F L A M M A B I L I TTYE S T

a) Timeof application of flame : 360 seconds


b) Lengthof the unaffected portionof cable
fromthe bottomof the too ' Sclamo
peciiieO
: 50mm (min)
Observed : 332 mm
c) Timeof burningafterremovalof flame
Specified : 60 seconds(max)
Observed : Extinguished
lmmediately

d) Conclusion: The specimenmeets the requirementsof the specification

T E S TE N G I N E E R
CABLES LABORATORY
D IA GN OS T ICCABLES
, & CAPACITORSDIVISION
C E N T R A LPOW ERRESEARCHINSTITUTE
P.B.No.8066,SADASIVANAGAR SUB P.O.
PROF.SIRC.V.RAMAN R O A D, B A N G A L O R E . 5 6O
0 B OI ,N D I A . NABLAccredited
CPRI Phone +91 (0) 80-23604435, Fax : +9'l (0) B0- 23601213 Laboratory
Cert.No T-0010

S h e e t1 0 o f 1 0
TESTREPORT

CPRI Test ReportNo.: DCCD-9l49 Date:08.08.2006

NOTE

al The Test resultsrelateonlyto the item(s)tested.

b ) Publicationor reproductionof thisreportin anyformotherthanby completeset of thewholereportand


in the languagewritten,is not permitted withoutthe writtenconsentof cpRl.

c) Any Corrections/erasure
invalidatesthistestreport.

d) Any anomaly/discrepancy
in thistestreportshouldbe broughtto our noticewithin45 daysfromthe date
of rssue.

e) The verification
of the sampledrawingsby CPRIis limitedto dimensional
checkingonlywherever
possible.

f) # indicates
thatthereis no formal NABLaccreditation
and however,the testsare conductedas per
relevantapplicable
National/lnternational
standardor as perthe specificcustomerrequirement.

C\-rt[
(Thirumurthf
),
T E S TE N G I N E E R
CABLES LABORATORY
CABLES& CAPACITORSDIVISION
DIAGNOSTIC,
CENTRALPOWERRESEARCHINSTITUTE
P.B.NO.8066,SADASIVANAGAR SUBP'O.
C.V.RAMAN ROAD,BANGALORE - 560O8O'INDIA' NABLAccredited
PROF.SIR
Fax
Phone: +91(0) 80-23604435, : +91(0) 80- 23601213
CPRI c",tNlfTS"d?ry
Client of lndiaLtd.,Mumbai
M/sCableCorporation
TestReport No.& Date DCCD-9149 Dated 08.08.2006
SampleCode DCCDCABO6SO5ST
Core Red

No, I
?4.n,06I
sll:LI
u P 'l6r
Tl' L l
1z' Jt.l
HJI]iv:1008
Tri€er: Int.
flogilfier,OFI
i fMir:1080. $2r oFt
i Triggr:Int

I'lo. l! l1o, IB
24.07.86 1 ?4,W ,0$
Oll: LI 0ll:LI
,
Ur, lZS' il-p , - l 0 J
" Tl' t't
t.
1' 2c *2 Tl' 1 ,
1 ? ,J I ,

l.UDiv:l00B
. Ol2: oFF Triger:Int

IHZ:fF

60 Jrs fl
CABLES LABORATORY
DIAGNOSTIC,
CABLES& CAPACITORSDIVISION
CENTRALPOWERRESEARCHINSTITUTE
P.B. No.8066,SADASIVANAGAR SUB P.O.
PROF.SIRC.V.RAMANROAD , BANGALORE- 560 O8O,INDIA. NABLAccredited
CPRI Phone. +91 (0) 80-23604435,Fax : +91 (0) 80 - 23601213
c",.il.l3bf6tt?u
Client M/s CableCorporationof IndiaLtd.,Mumbai
Test Report No.& Date DCCD-9149Dated08.08.2006
SampleCode DCCDCABO6SOs8T
Core Yellow

l1o, I
?4,W,961
Oil:LI
284 U": -170,
f

Tz' 51'Bl Tl' l'l


KU
T z '5 l '
150 KEiv, lB0B
Trigger: In
f l o m i fi r : 0
fMJiu:
Ol2:cFF Int
Trigger:
fi

01?,OFF

llo. I B
No, l0 24.97.gEI
z4.E7.gEI Sll, LI
tll: LI U- : -l7B
Tl' l'
Iz' 5l'

lfJlli uI
Tr igger I n t

012:oFF

TEST ENGINEER
CABLES LABORATORY
CABLES& CAPACITORSDIVISION
DIAGNOSTIC,
CENTRALPOWERRESEARCHINSTITUTE
P.B. No.8066,SADASIVANAGAR SUB P'O'
PROF.SIRC"V.RAMAN'ROAD, BANGALORE'560 O8O'INDIA NABLAccredited
fat : +91 (0) 80 - 23601213
pnone : +91 (0) eO-2gOO+ag6,
CPRI c"'.til8T6tt?Y
Client M/s Cable Corporationof India Ltd', Mumbai
TestReport No-& Date DCCD-9149Dated08'08'2006
SampleCode DCCDCABO6SOsST
Core Blue

No, I
l1o, I
?4.87.06| ?4,87,06I
Oll: LI Sll:Li
u-: 169' , P ,-l7g,
Tr l'
T l' l , l
T 2 ' 5 8
1?'

1000'
lf.,[iu:
Triqqer' lnt
iloqilfier,ff
012,ffF

60 rs S0

l'lo, l0
24.I7.86
No,l0 &llr LI
?4.w,gE u- : -169
Sll:LI
ri r.l
U": 168 T2' 58'
f

' ' ' "T l ' 1'


T2'51 llJ[iv:
T r i g g c r :I n t

'
flJliv:1008 Sl2: OFF
Trigger:Inl

{\ ^rt[\
$w{5t
(Thirumurthy) I ,
TEST ENGINEER
@)
M DIELECTRICS MATERIALS DIVISION
INSULATION LABORATORY
CPRI CENTRAL POWER RESEARCH INSTITUTE NABLAccredited
Sir C.V. RamanRoad,p.B.NO.g066,BANGALORE_560 0g0
Laboratory
Phoneno. 3602919Ext 239112393
Fax:080_23
601213

SheetI of3

T E S TR E P O R T
Test ReportNumUer Oatect
INS/M/oo3/J
ur_yloo_oz
orZZlz oo
Name& Addressot ttretlient
M/s-CabteCorpora-ionGGoiaTtd,
D_attapada
Road,Borivili(East),
ffi !lumbai-400066
DcCDretter
ruoZgloecblOant
d t . 11 . 0 7 . 0 6
ut [ne Manuracturer M/s.CableCorporation oitnOiaL[
Mumbai
Lruurarsor sample tested/calibrated -
\rdrv.rntseQ sleetTormed
wirearmourof 3 x
400Sq.mm,Aluminium conductor,XLpE
insulated, PVCsheathed, Galvanisedsteel
--
r lormedwirearmoured19/33kV Cabte.
raurpte 0n Kecelpt Received in goodcondrtion
Type
-
-
-
Numberof sambtEs
tested -
ut Lcst(s/
:as\D,t 27.07.06
urKt samptecodeno
-=-
9^tt^ttl^F- ^, +^^. ---

Tensitestre@
T. avcv{ r i
armour
,,, qvvv,
vqr rue wrU I srdnuaro/spgclllcatlon
_- AspertST0gSpt.m
SamEnfitan
- '
::: :
Client'srequirement-
Nii-

Client'srepreseffi
None
None
I cruv.lrorauon suDcontracted
with addressof the NA
laboratory
uuuuurenrs constrtutrng this report (in
words)
Three
Nil-
Nil
Nil
Nil
Nil

iutln-t*\,/rtJ\
' \--
\
(Dr.K.Dwdlakanath)
T E S TE N G I N E E R
ADDITIONALDIRFeToP
&LiT?3
* W,,
&Xmffi,e ?"t
fAT* etn%
t@)
M DIELECTRICS MATERIALS DIVISION
INSULATION LABORATORY
NABLAccredited
CENTRAL POWER RESBARCH INSTITUTE
CPRI Sir C.V. RamanRoad,P.8.NO.8066, BANGALORE-5600g0
Laboratory
Phoneno. 36029| 9 Ext 239| I 2393Fax:080-23601213

Sheet2 of 3

Continuationof Test
INS/M/003/JULy/06-07
dt.22.07 .06
M/s.CableCorporation
of IndiaLtd.,
DattapadaRoad,Borivili(East),
Mumbai-400 066
Galvanised
steelformedwirearmourof 3 x 400
Sq.mm,Aluminium conductor, XLpEinsulated,
PVCsheathed, Galvanised steelformedwire
armoured 19/33kV Cable.
DCCDCAB06S0587

Laboratoryconditions:
Laboratory
temperature :25t2 "C
RelativeHumidity : 65*5 %

TestParametersfor Tensilestrengthand Elongation:

Instrumentused UniversalTestingMachine
Number of specimen Three
Loadcell 5000N,Rangesetected: 2000N
Speed 100mm/min
Gaugelength 2 5 0m m
Conditioning Tested'as in received
condition'
Samplepreparation Samplesstraightened by tappingwitha woodennammer.

TESTRESULTS

Sl.No TESTSCONDUCTED RESULTS


OBTAINED SPECIFIED
VALUES
1 Tensilestrength
(MPa) 472.96 Between
300& 500MPa
Elongation
at break(%) 4 4 E,E
1 0 %( m i n )

conclusion:
Resultsmeetthe requirements
of the specification.

.. . i ,',. .t-"
. <^ .- ii

(Dr.C.Viswanatha) .:
T E S TE N G I N E E R
DIELECTRICS MATERIALS DIVISION
INSULATION LABORATORY
NABLAccredited
CPRI CENTRAL POWER RESEARCHINSTITUTE
Sir C.V. RamanRoad,P.8.NO.8066,BANGALORE-560080
Laboratory
Phoneno. 3602919Ext239ll2393Fax:080-23601213

Sheet3 of 3

Continuationof Test
INS/M/003/JULy/o6-07dt.22.07 .06
M/s.CableCorporation of IndiaLtd.,
DattapadaRoad,Borivili(East),
Mumbai-400 066
Galvanisedsteelstriparmourof 3 x 400Sq.mm,
Aluminiumconductor, XLPEinsulated, PVC
sheathed,Galvanised steelformedwirearmoureo
19/33kV Cables.
DCCDCABO6SO5ST

NOTE
a) Thetestresultsrelateonlyto the item(s)tested.

b) Publicationor reproduction of this reporVcertificate


in any form otherthan by
completeset of the wholereportand in the languagewritten,is not permitted
withoutthe writtenconsentof CPRI.

c) Any correction/erasure
invalidates
thistestreporucertificate.

d) Any anomaly/discrepancy in this test reporUcertificate


shouldbe broughtto our
noticewithin45 daysfromthedateof issue.

e) The verification
of the sampledrawingsby CPRIis limitedto dimensional
checks
onlywhereverpossible.

f) # Markindicatesthatfor suchteststhereis no formalNABLaccreditationandthe


testsare conducted as perthe relevant
applicablenational/international
standard
or as perspecificcustomerrequirement.

r , ' t ' r . , t . r . . . . i c
(Dr.C.ViswanathEfr-
TESTENGINEER

You might also like