Ref.

No JSPL/ANGUL/TDC-004976A
TECHNICAL DELIVERY CONDITIONS
Rev. 1
TSD-PLATE DIVISION FOR HOT ROLLED PLATES
ANGUL-ODISHA(INDIA) Date of Issue 20/07/2023
Customer Name : METSO OUTOTEC INDIA PRIVATE LIMITED

1 Grade and Specification IS 2062 E250 BR


2 Process Route BF>BOF/ EAF>LRF>VD>SLABCASTER>RHF>HOT ROLLING
3 Supply Condition Normalizing Rolling
4 Steel making practice Fully Killed
5 End Uses Structural Purpose
6 Chemical Composition Raw Material Grade
Ladle Analysis
Elements Thickness, t (mm) Internal Grade
Min Max
8.0 - 150.0 8.00 <= t <= 18.00 :
%C 0.22 JA25STTM01N
%Mn 1.50 18.01 <= t <= 40.00 :
%S 0.045 JA25STTMN02

%P 0.045 40.01 < t <= 79.99 :


JA25STTMN03
%Si 0.03 0.40
%Al 0.010 80.00 <= t <= 99.99 :
JA25STN04
%(V+Nb+Ti) 0.25
100.00 <= t <= 150.00 :
%N 0.012
JA25STN05
%CE(IIW) 0.41

Chemical Remarks
CE(IIW) = C+Mn/6+(Cr+Mo+V)/5 +(Ni+Cu)/15
7
Mechanical Properties
Elongation (%) Thick (mm) Bend Test (180°)
Thick (mm) YS (MPa) UTS (MPa)
(min) Internal
Sample
Sample GL=5.65 So Min Max Mandrel
Min Max Min Min Orientation
Orientation (mm) Diameter
8 19.99 T 250 410 23 8 25 T 2t
20 40 T 240 410 23 40.01 150 T 3t
40.01 150 T 230 410 23
CVN Impact Test
Temp Energy (J) Energy (J) Sample
(°C ) (minimum individual) (minimum average) Orientation
25 19 27 L

T: Transverse direction L: Longitudinal direction { CVN Impact test:1sample =3 specimens}

Note 1 Speed of tensile testing:


Rate of stress/ strain to be followed as below
As per IS 1608 CL. No. 10.3.3.2 & 10.3.3.3
- For Yield properties: 6 MPa / s to 60 MPa / s
- For Tensile properties: max strain rate 0.008 / s, but not less than test speed of the yield range.

8
Test Sample Frequency in as supplied condition
Tensile Bend Impact
2 samples per 2 samples per 1 sample per
heat heat heat

9
Other Details
Dimensional Tolerance
TolThickness (mm) TolLength Edge Condition

Doc no.: REC-PM-TSD-01-06, Rev. No. 00, Effective Date - 28.10.2020 1


Ref.No JSPL/ANGUL/TDC-004976A
TECHNICAL DELIVERY CONDITIONS
Rev. 1
TSD-PLATE DIVISION FOR HOT ROLLED PLATES
ANGUL-ODISHA(INDIA) Date of Issue 20/07/2023
Customer Name : METSO OUTOTEC INDIA PRIVATE LIMITED

As per EN 10029 Class A -0/+50 mm Mill Edge

Edge Condition Description

i.Customer shall trim plate edges up to 1.5 X thickness or 40 mm, whichever is maximum, on each edge of the plates.
ii. Width Tolerance for plates with Mill edge condition

Width ( w ) Width Tolerance


w <= 2500 mm - 0 / + 60 mm
2500 < w <= 3000 mm - 0 / + 80 mm
3000 < w <= 3500 mm - 0 / + 90 mm
3500 < w <= 4000 mm - 0 / + 110 mm

iii. JSPL will not do grinding near the plate edges (refer point i) for any surface imperfections.
iv. Customer / Customer's Representative will not hold any plate if any defect is observed near the edges (refer point i).

Edge Camber Out Of Squareness Flatness

Maximum 0.2% of the actual length Maximum 1% of the actual width As per EN 10029 Class N Type L

Plate Inspection
Ultrasonic Inspection Visual Inspection

EN10160 S1E1
Surface quality: As per IS 2062 Clause 7.1 and 7.2. Repair by
Inspection will be carried out from one Major Surface of the plate, welding shall not be done.
preferably from Top Surface only.

Test Certificate Packing Condition

As per EN 10204: 3.1 Loose condition

9
Plate Marking
Stencil Marking Hard Punching
Manufacture's Name Yes
Heat No. /Plate No. Yes Yes
Grade/Specification Yes Yes
Size (Thickness x Width x Length) (in mm) Yes
UT Level Yes

Plate Marking Remarks

Stenciling + hard punching shall be done on top surface of the plate at one end.

11
Inspection Agency
By JSPL

12
Remarks

1.Any handwritten modification / comment in this document will make this document invalid and shall need reconfirmation from Plant.
2. Steel is a technical product and any guarantee regarding the end application shall not come under JSP's obligations. JSP shall fulfill the properties as
defined in this TDC only.

Doc no.: REC-PM-TSD-01-06, Rev. No. 00, Effective Date - 28.10.2020 2


Ref.No JSPL/ANGUL/TDC-004976A
TECHNICAL DELIVERY CONDITIONS
Rev. 1
TSD-PLATE DIVISION FOR HOT ROLLED PLATES
ANGUL-ODISHA(INDIA) Date of Issue 20/07/2023
Digitally signed by Anshul Jain
Customer Name : METSO OUTOTEC INDIA PRIVATE LIMITED Anshul DN: cn=Anshul Jain, c=IN,
o=Metso Outotec India Pvt. Ltd.,
email=anshul.jain@mogroup.com

Initiator Approved By
Jain Date: 2023.08.21 08:44:48
+05'30'
Customer Approved
Prepared By Reviewed By Section incharge(TSD) (Seal & Signature)

Doc no.: REC-PM-TSD-01-06, Rev. No. 00, Effective Date - 28.10.2020 3

You might also like