Professional Documents
Culture Documents
CT22-2099-WQ22-2099-Plant Trial Mix-C 40 OPC-17-07-2022
CT22-2099-WQ22-2099-Plant Trial Mix-C 40 OPC-17-07-2022
Mix Description Characteristic Strength : 40 MPa (Cyl) Total Cl & SO3 as % of Cement
3
C40 (410kg/m ) OPC+8%MS W/CM : 0.38 Chlorides (Cl) : 0.05
200±40MM SLUMP Cementitious Content : 410 Kg/m3 Sulphate (SO3) : 2.7
Slump : 200 mm
\
Specific Absorbed
MATERIAL DETAILS Weights B. Down% Source 3
Cl% SO3% Absn.%
Gravity Vol. m Water
CEM 1 OPC kg. 377 92 Yamama/RCC 3.15 0.120 2.66
CEM 2 MS kg. 33 8 Ferro Altlantica 2.20 0.015
CEM 3 kg. 0 Ferro Altlantica 2.20 0.000
Additive kg.
Free Water ltr. 155 Local 1.00 0.155 0.001 0.0011
40mm kg. 2.70 0.000
20mm kg. 700 38.5 Rumah/Haradh 2.63 0.266 0.017 0.017 1.43 10.0
10mm kg. 370 20.3 Rumah/Haradh 2.62 0.141 0.009 0.009 1.54 5.7
0-5mm kg. 270 14.8 Rumah/Haradh 2.64 0.102 0.007 0.007 1.64 4.4
0 - 1 Dune Sand kg. 480 26.4 Shaqra/Kharj 2.62 0.183 0.012 0.012 0.72 3.5
Admix.1STRW420TG5/Equiv. ltr. 3.0 - 7.0 FOSROC/DCP 1.06
Admix.2 MP 389/Equiv. ltr. 0.5 - 5.0 BASF/DCP 1.09
Admix.3 ltr.
Air % 2 0.0200
Remarks:
-Making, Curing and Testing of specimens shall be in accordance with BS/BSEN/ASTM Standards.
-The above mentioned admixture dose is for average ideal dose; it will vary as per working conditions to maintain required workability and setting
time, but within the manufacturer recommended dosages.
-Extra Admixture will be added on site to control workability if necessary.
-The strength indicated above is Cylinder Strength at 28days.
TGRMCC reserve the right to adjust these mixes any time with the approval from consulting engineer, justified changes in accordance with TGRMCC Quality
Control & Assurance Programme