Sagarmatha Precast solutions Pvt.

Ltd
Sunwal-9 swathi

LABORATARY REPORT FOR COMPRESSIVE STRENGTH TEST OF CONCRETE PAVERS

Paver type: Rectangular paver


paver colour: Grey colour
Height of paver: 60 mm
PAVER TEST REPORT
Paver Casting Date:11-02-2024
Age of paver at test 28 days
concrete grade M35
Date of testing 10/3/2024
Paver number No. 1 2 3
Length of paver,L M 0.2 0.2 0.2
Bredth of paver,B M 0.1 0.1 0.1
Height of paver,H M 0.06 0.06 0.06
Volum of paver:(LxBxH) M 0.0012 0.0012 0.0012
Density of paver (G=W/V) Kg/m3 2266.67 2158.33 2266.67
Surface Area of paver(A) mm2 20000 20000 20000
Weight of paver,(W) Kg 2.72 2.59 2.72
Maximum Load,(P) KN 794.6 781 772.2
Paver strength=(M/LXB)X1000 N/mm2 39.73 39.05 38.61
Average paver strength N/mm2 39.13
TEST RESULT:
Description Specification Actual value
curing period 28 days 28 days PASS
Compressive Strength 35 39.13
Tested by :Krishana chaudhary